AWS B2.1/B2.1M-BMG:2009
Base Metal Grouping for Welding Procedure and Performance Qualification
AWS B2.1/B2.1M-BMG:20...
91 downloads
1484 Views
617KB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
AWS B2.1/B2.1M-BMG:2009
Base Metal Grouping for Welding Procedure and Performance Qualification
AWS B2.1/B2.1M-BMG:2009
Base Metal Grouping for Welding Procedure and Performance Qualification Prepared by the American Welding Society (AWS) B2 Committee on Procedure and Performance Qualification Under the Direction of the AWS Technical Activities Committee Approved by the AWS Board of Directors
Abstract This document provides the AWS base metal grouping for welding procedure and performance qualification and is identical to Annex D of AWS B2.1/B2.1M:2009, Specification for Welding Procedure and Performance Qualification.
550 N.W. LeJeune Road, Miami, FL 33126
AWS B2.1/B2.1M-BMG:2009
International Standard Book Number: 978-0-87171-748-1 American Welding Society 550 N.W. LeJeune Road, Miami, FL 33126 © 2009 by American Welding Society All rights reserved Printed in the United States of America Photocopy Rights. No portion of this standard may be reproduced, stored in a retrieval system, or transmitted in any form, including mechanical, photocopying, recording, or otherwise, without the prior written permission of the copyright owner. Authorization to photocopy items for internal, personal, or educational classroom use only or the internal, personal, or educational classroom use only of specific clients is granted by the American Welding Society provided that the appropriate fee is paid to the Copyright Clearance Center, 222 Rosewood Drive, Danvers, MA 01923, tel: (978) 750-8400; Internet: <www.copyright.com>.
ii
AWS B2.1/B2.1M-BMG:2009
Statement on the Use of American Welding Society Standards All standards (codes, specifications, recommended practices, methods, classifications, and guides) of the American Welding Society (AWS) are voluntary consensus standards that have been developed in accordance with the rules of the American National Standards Institute (ANSI). When AWS American National Standards are either incorporated in, or made part of, documents that are included in federal or state laws and regulations, or the regulations of other governmental bodies, their provisions carry the full legal authority of the statute. In such cases, any changes in those AWS standards must be approved by the governmental body having statutory jurisdiction before they can become a part of those laws and regulations. In all cases, these standards carry the full legal authority of the contract or other document that invokes the AWS standards. Where this contractual relationship exists, changes in or deviations from requirements of an AWS standard must be by agreement between the contracting parties. AWS American National Standards are developed through a consensus standards development process that brings together volunteers representing varied viewpoints and interests to achieve consensus. While the AWS administers the process and establishes rules to promote fairness in the development of consensus, it does not independently test, evaluate, or verify the accuracy of any information or the soundness of any judgments contained in its standards. AWS disclaims liability for any injury to persons or to property, or other damages of any nature whatsoever, whether special, indirect, consequential, or compensatory, directly or indirectly resulting from the publication, use of, or reliance on this publication. AWS also makes no guarantee or warranty as to the accuracy or completeness of any information published herein. In issuing and making this publication available, AWS is neither undertaking to render professional or other services for or on behalf of any person or entity, nor is AWS undertaking to perform any duty owed by any person or entity to someone else. Anyone using these documents should rely on his or her own independent judgment or, as appropriate, seek the advice of a competent professional in determining the exercise of reasonable care in any given circumstances. It is assumed that the use of this standard and its provisions are entrusted to appropriately qualified and competent personnel. This publication may be superseded by the issuance of new editions. Users should ensure that they have the latest edition. Publication of this document does not authorize infringement of any patent or trade name. Users of this publication accept any and all liabilities for infringement of any patent or trade name items. AWS disclaims liability for the infringement of any patent or product trade name resulting from the use of this publication. Finally, AWS does not monitor, police, or enforce compliance with this publication, nor does it have the power to do so. On occasion, text, tables, or figures are printed incorrectly, constituting errata. Such errata, when discovered, are posted on the AWS web page (www.aws.org). This publication is subject to revision at any time by the AWS B2 Committee on Procedure and Performance Qualification. Comments (recommendations, additions, or deletions) and any pertinent data that may be of use in improving this publication are required and should be addressed to AWS Headquarters. Such comments will receive careful consideration by the AWS B2 Committee on Procedure and Performance Qualification and the author of the comments will be informed of the Committee’s response to the comments. Guests are invited to attend all meetings of the AWS B2 Committee on Procedure and Performance Qualification to express their comments verbally. Procedures for appeal of an adverse decision concerning all such comments are provided in the Rules of Operation of the Technical Activities Committee. A copy of these Rules can be obtained from the American Welding Society, 550 N.W. LeJeune Road, Miami, FL 33126.
iii
AWS B2.1/B2.1M-BMG:2009
This page is intentionally blank.
iv
AWS B2.1/B2.1M-BMG:2009
Personnel AWS B2 Committee on Procedure and Performance Qualification J. J. Fluckiger, Chair J. L. Cooley, 1st Vice Chair E. W. Beckman, 2nd Vice Chair S. Morales, Secretary L. P. Connor W. D. Doty E. H. Gray B. J. Hable M. Herrle R. A. LaFave K. Y. Lee K. M. McTague A. S. Olivares J. F. Pike W. M. Ruof J. J. Sekely M. R. Stone G. M. Wisbrock R. K. Wiswesser
Idaho National Laboratory J. C. and Associates, Incorporated International Training Institute American Welding Society Consultant Doty and Associates, Incorporated U.S. Nuclear Regulatory Commission Ford Motor Company Arise, Incorporated Elliott Company, Incorporated The Lincoln Electric Company Factory Mutual HSB Global Standards NASA Langley Research Center Bechtel Plant Machinery, Incorporated Welding Services, Incorporated Canadian Welding Bureau Lockheed Martin Missiles and Fire Control (Retired) Welder Training and Testing Institute
Advisors to the AWS B2 Committee on Procedure and Performance Qualification W. L. Ballis J. D. Duncan N. K. Kanaya B. B. MacDonald A. W. Sindel C. E. Speader, Jr. W. J. Sperko R. F. Waite
Consultant Consultant BEAR Testing Laboratory Consultant Alstom Power—USA Aristech Chemical Corporation Sperko Engineering Services Consultant
AWS B2A Subcommittee on Brazing Qualification J. L. Cooley, Chair S. Morales, Secretary J. J. Fluckiger L. Guimaraes R. A. LaFave R. L. Peaslee W. J. Sperko K. P. Thornberry G. M. Wisbrock R. K. Wiswesser
J. C. and Associates, Incorporated American Welding Society Idaho National Laboratory National Automotive Corporation Elliott Company Wall Colmonoy Corporation Sperko Engineering Services Care Medical, Incorporated Lockheed Martin Missiles and Fire Control (Retired) Welder Training and Testing Institute
v
AWS B2.1/B2.1M-BMG:2009
Advisors to the AWS B2A Subcommittee on Brazing Qualification W. D. Rupert J. J. Sekely C. E. Spaeder
Wolverine Joining Technologies Welding Services, Incorporated Consultant
AWS B2B Subcommittee on Welding Qualification G. M. Wisbrock, Chair S. Morales, Secretary E. W. Beckman L. P. Connor J. L. Cooley W. D. Doty J. J. Fluckiger E. H. Gray B. J. Hable K. Y. Lee K. M. McTague A. S. Olivares J. F. Pike J. J. Sekely M. R. Stone R. K. Wiswesser
Lockheed Martin Missiles and Fire Control (Retired) American Welding Society International Training Institute Consultant J. C. and Associates, Incorporated Doty and Associates, Incorporated Idaho National Laboratory U.S. Nuclear Regulatory Commission Ford Motor Company The Lincoln Electric Company Factory Mutual HSB Global Standards NASA Langley Research Center Welding Services, Incorporated Canadian Welding Bureau Welder Training and Testing Institute
Advisors to the AWS B2B Subcommittee on Welding Qualification W. L. Ballis J. D. Duncan N. K. Kanaya V. A. McCray A. W. Sindel W. J. Sperko
Consultant Consultant BEAR Testing Laboratory ExxonMobil Research and Engineering Company Sindel and Associates Sperko Engineering Services
AWS B2C Subcommittee on Materials W. M. Ruof, Chair S. Morales, Secretary W. D. Doty J. J. Fluckiger M. Herrle R. A. LaFave
Bechtel Plant Machinery, Incorporated American Welding Society Doty and Associates, Incorporated Idaho National Laboratory Arise, Incorporated Elliott Company, Incorporated
Advisors to the AWS B2C Subcommittee on Materials C. E. Cross A. Donlevy G. L. Hoback B. Moore P. Pollak A. P. Seidler A. W. Sindel C. E. Speader, Jr. L. T. Vernam G. M. Wisbrock
Federal Institute for Material International Titanium Association Haynes International Spectrulite Aluminum Association Armco Steel Sindel and Associates Aristech Chemical Corporation AlcoTec Wire Corporation Lockheed Martin Missiles and Fire Control (Retired)
vi
AWS B2.1/B2.1M-BMG:2009
AWS B2D Subcommittee on Standard Welding Procedure Specifications J. J. Sekely, Chair S. Morales, Secretary L. P. Connor W. D. Doty J. J. Fluckiger K. M. McTague W. M. Ruof
Welding Services, Incorporated American Welding Society Consultant Doty and Associates, Incorporated Idaho National Laboratory Factory Mutual Bechtel Plant Machinery, Incorporated
Advisor to the AWS B2D Subcommittee on Standard Welding Procedure Specifications G. M. Wisbrock
Lockheed Martin Missiles and Fire Control (Retired)
AWS B2E Subcommittee on Soldering Qualification E. W. Beckman, Chair S. Morales, Secretary J. L. Cooley J. J. Fluckiger E. H. Gray P. T. Vianco
International Training Institute American Welding Society J. C. and Associates, Incorporated Idaho National Laboratory U.S. Nuclear Regulatory Commission Sandia National Laboratories
Advisors to the AWS B2E Subcommittee on Soldering Qualification G. M. Wisbrock R. Zahner
Lockheed Martin Missiles and Fire Control A Zahner Company
AWS B2F Subcommittee on Plastic Welding Qualification L. T. Hutton, Chair R. Hanselka, Vice Chair S. P. Hedrick, Secretary K. Argasinki R. Basile M. Callahan D. Chandler J. Craig P. Demchko J. J. Fluckiger S. M. Gardiner D. P. Glavin G. Hopkins J. Leary B. B. MacDonald P. F. Martin C. L. Parker G. Sample J. Sciadini K. C. Thomas M. J. Troughton D. Ziegler P. Zitkus
ARKEMA, Incorporated Advanced Industrial Design American Welding Society Solvay Solexis AB Plastics, Incorporated Local 290 Engiplast, Incorporated McElroy Manufacturing, Incorporated Solvay Solexis Idaho National Laboratory IPS Corporation Steamfitters Local Union 449 Plastek Werks, Incorporated Asahi American, Incorporated Consultant United Association Lubrizol Advanced Materials, Incorporated George Fischer Tech South, Incorporated Quadrant EPP TWI Wegener North America, Incorporated Wegener Welding
vii
AWS B2.1/B2.1M-BMG:2009
Advisors to the AWS B2F Subcommittee on Plastic Welding Qualification J. Hessel R. James A. Lopez G. M. Wisbrock
Hessel Ingenieurtechnik GmbH International Training Institute Dow Chemical Lockheed Martin Missiles and Fire Control (Retired)
viii
AWS B2.1/B2.1M-BMG:2009
Table of Contents Page No. Personnel ......................................................................................................................................................................v 1. Scope ......................................................................................................................................................................1 Annex D—Base Metal Grouping .................................................................................................................................3
List of Tables Table D.1 D.1 D.2 D.2 D.3
Page No. Listing of Base Metal Specifications—Ferrous Alloys .................................................................................4 Listing of Base Metal Specifications—Nonferrous Alloys .........................................................................42 M-Number Listing of Base Metals—Ferrous Alloys...................................................................................66 M-Number Listing of Base Metals—Nonferrous Alloys...........................................................................131 Listing of Base Metal Specifications—Iron Castings................................................................................189
ix
AWS B2.1/B2.1M-BMG:2009
This page is intentionally blank.
x
AWS B2.1/B2.1M-BMG:2009
Base Metal Grouping for Welding Procedure and Performance Qualification 1. Scope This publication is an extract of AWS B2.1, Specification for Welding Procedure and Performance Qualification, and is identical to Annex D, Base Metal Grouping, in the 2009 edition of that standard. This publication supersedes AWS B2.1-BMG:2005. Underlined text or a vertical line in the margin indicates a revision from the 2005 edition. This publication may be referred to by other codes and standards that have welding procedure and performance requirements in order to avoid duplication of materials tables in those publications. Base metals and filler metals have been grouped into categories that will minimize the number of qualification tests required. Substitution of one base metal or filler metal for another, even when within the allowable rules, should only be made after an evaluation of the factors involved. For some materials, additional tests may be required. Materials not listed require separate qualification.
1
AWS B2.1/B2.1M-BMG:2009
This page is intentionally blank.
2
AWS B2.1/B2.1M-BMG:2009
Annex D (Normative) Base Metal Grouping This annex is part of AWS B2.1/B2.1M:2009, Specification for Welding Procedure and Performance Qualification, and includes mandatory elements for use with this standard.
D1. Base Metal Specifications
D2. Material Number (M-Number) Groupings
Table D.1 indexes ASTM, ABS, API, AISI, AS, AS/NZS, CSA, AMS, ISO, NACE, and MSS base metals in numerical order to provide ease of reference when determining into what grouping a particular base metal specification falls.
Base metal has been divided into general categories, e.g., Material Numbers (M-Numbers) 1, 1A, 3, 3A, 4, 4A, etc., and further divided into groups within each general category. The category grouping does not imply that base metals may be substituted for other base metals within the same Material Number (M-Number) without consideration for weldability.
Table D.2 groups base metals for welding procedure and performance qualification on the basis of mechanical properties, chemical composition, and metallurgical compatibility to minimize the number of welding qualification where this can logically be done.
D3. Iron Castings Specifications Base metal specifications for iron castings are divided into D11.2 groups.
3
AWS B2.1/B2.1M-BMG:2009
Table D.1 List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K03100 K02595 K02596 K02597 K02598 K02599 K02600 K02504 K03005 — K02504 K03005 K03504 K02501 K03006 K03501 G10150 G10180 G10200 K02300 K02102 K01601 K02101 K01601 K01801 K11846 K11852 K11846 K11852 K11846 K11852 — — — K02401 K02702 K01700 K02200 K02801 — — — K03003
Rivets Plate Plate & Bars Plate & Bars Plate & Bars Plate & Bars Shapes Resistance Welded Pipe Resistance Welded Pipe Furnace Welded Pipe Seamless Pipe Seamless Pipe Pipe Flanges Seamless Pipe Seamless Pipe Seamless Pipe Bar Bar Bar Structural Structural Structural Structural Structural Structural Structural Structural Structural Structural Structural Structural Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe ERW Pipe ERW Pipe Welded Pipe Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 31 A 36 A 36 A 36 A 36 A 36 A 36 A 53 A 53 A 53 A 53 A 53 A 105 A 106 A 106 A 106 A 108 A 108 A 108 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 134 A 134 A 134 A 134 A 134 A 134 A 134 A 134 A 135 A 135 A 139 A 139
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 2 1 1 2 1 1 1 1 1 1 1 1 2 2 2 2 2 2 2 1 1 1 1 1 1 1 1 1 1 1 1
Grade B A36 A36 A36 A36 A36 A36 Type E, Grade A Type E, Grade B Type F, Grade A Type S, Grade A Type S, Grade B — Grade A Grade B Grade C Grade 1015 CW Grade 1018 CW Grade 1020 CW Grade A Grade B Grade CS Grade D Grade DS Grade E Grade AH32 Grade AH36 Grade DH32 Grade DH36 Grade EH32 Grade EH36 A36 A283 A A283 B A283 C A283 D A285 A A285 B A285 C Grade A Grade B Grade A Grade B (Continued)
4
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K03004 K03010 K03012 — K11522 K01504 S30800 S30900 S30908 S31000 S31008 K01200 K03503 — K01200 K03502 K03502 K12122 K12822 K11562 K11564 K11572 K11572 K11597 K21590 K21590 K31545 K41545 K42544 K90941 K90901 K31830 S41000 S42900 S41000 S41000 S41000 S41026 S41500 S43000 S30400 S30403 S30409
Welded Pipe Welded Pipe Welded Pipe Castings Tube Low C Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip ERW Tube ERW Tube ERW Tube Seamless Tube Pipe Flanges Pipe Flanges Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 139 A 139 A 139 A 148 A 161 A 161 A 167 A 167 A 167 A 167 A 167 A 178 A 178 A 178 A 179 A 181 A 181 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182
1 1 1 4 3 1 8 8 8 8 8 1 1 1 1 1 1 3 3 4 4 4 4 4 5A 5A 5A 5B 5B 5B 5B 5C 6 6 6 6 6 6 6 7 8 8 8
1 1 1 3 1 1 2 2 2 2 2 1 1 2 1 1 2 2 2 1 1 1 1 1 1 1 1 1 1 1 2 1 1 2 3 3 3 3 4 2 1 1 1
Grade C Grade D Grade E Grade 90-60 Grade T1 Low Carbon Type 308 Type 309 Type 309S Type 310 Type 310S Grade A Grade C Grade D — Class 60 Class 70 Grade F2 Grade F1 Grade F12, Class 1 Grade F12, Class 2 Grade F11, Class 2 Grade F11, Class 3 Grade F11, Class 1 Grade F22, Class 1 Grade F22, Class 3 Grade F21 Grade F5 Grade F5a Grade F9 Grade F91 Grade F3V Grade F6a, Class 1 Grade F429 Grade F6a, Class 2 Grade F6a, Class 3 Grade F6a, Class 4 Grade F6b Grade F6NM Grade F430 Grade F304 Grade F304L Grade F304H (Continued)
5
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S30451 S30453 S30600 S31600 S31603 S31609 S31651 S31653 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S33100 S30815 S31000 S20910 S21904 S31254 K22035 S31200 S31803 S32750 S32760 S32205 S32550 S44627 K01201 K11597 K31545 K21590 K31509 K41545 K81590 S50460 K31545 K21590 K31509 K11742 K12542
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Flanges & Fittings Flanges & Fittings Flanges & Fittings Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Tube Tube Tube Plate Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 192 A 199 A 199 A 199 A 199 A 199 A 199 A 199 A 200 A 200 A 200 A 202 A 202
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 9A 10H 10H 10H 10H 10H 10H 10I 1 4 5A 5A 5A 5B 5B 5B 5A 5A 5A 4 4
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 3 3 4 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1
Grade F304N Grade F304LN Grade F46 Grade F316 Grade F316L Grade F316H Grade F316N Grade F316LN Grade F317 Grade F317L Grade F321 Grade F321H Grade F347 Grade F347H Grade F348 Grade F348H Grade F10 Grade F45 Grade F310 Grade FXM-19 Grade FXM-11 Grade F44 Grade FR Grade F50 Grade F51 Grade F53 Grade F55 Grade F60 Grade F61 Grade FXM-27Cb — Grade T11 Grade T21 Grade T22 Grade T4 Grade T5 Grade T9 Grade T91 Grade T21 Grade T22 Grade T4 Grade A Grade B (Continued)
6
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K21703 K22103 K30018 K31718 K32018 K11820 K12020 K12320 K11522 K12023 K11422 K02707 K03501 K11547 K11562 K11597 K21590 K31545 K41245 K41545 K51545 K90941 K90901 S30400 S30403 S30409 S30451 S30453 S31600 S31603 S31609 S31651 S31653 S32100 S32109 S34700 S34709 S34800 S34809 S38100 S30815 S30908 S30909
Plate Plate Plate Plate Plate Plate Plate Plate Seamless Tube Seamless Tube Seamless Tube Seamless Tube ERW Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 203 A 203 A 203 A 203 A 203 A 204 A 204 A 204 A 209 A 209 A 209 A 210 A 210 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213
9A 9A 9B 9B 9B 3 3 3 3 3 3 1 1 3 4 4 5A 5A 5B 5B 5B 5B 5B 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 2 2 1 1 1 1 2 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2
Grade A Grade B Grade F Grade D Grade E Grade A Grade B Grade C Grade T1 Grade T1a Grade T1b Grade A1 Grade C Grade T2 Grade T12 Grade T11 Grade T22 Grade T21 Grade T5c Grade T5 Grade T5b Grade T9 Grade T91 TP304 TP304L TP304H TP304N TP304LN TP316 TP316L TP316H TP316N TP316LN TP321 TP321H TP347 TP347H TP348 TP348H Grade XM-15 TP253MA TP309S Type 309H (Continued)
7
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S30940 S30941 S31000 S31008 S31009 S31040 S31041 S31050 S20100 S20200 S31725 S31726 K12047 K01807 J02502 J03002 J02503 J12524 J12082 J22000 J12072 J21890 J82090 J42025 J84090 J91150 K12524 — K01201 K03006 K03501 K12821 — K12062 — — K12062 K21590 K21590 K41545 K90941 S50460 K22035
Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube ERW Tube Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Plate Plate ERW Tube Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 214 A 216 A 216 A 216 A 217 A 217 A 217 A 217 A 217 A 217 A 217 A 217 A 217 A 225 A 225 A 226 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234 A 234
8 8 8 8 8 8 8 8 8 8 8 8 10B 1 1 1 1 3 4 4 4 5A 5B 5B 5B 6 10A 10A 1 1 1 3 4 4 4 4 4 5A 5A 5B 5B 5B 9A
2 2 2 2 2 2 2 2 3 3 4 4 1 1 1 2 2 1 1 1 1 1 1 1 1 3 1 1 1 1 2 1 1 1 2 2 2 1 1 1 1 2 1
TP309Cb Type 309HCb Type 310 TP310S Type 310H TP310Cb Type 310HCb TP310MoLN TP201 TP202 TP317 LM TP317LMN Grade T17 — Grade WCA Grade WCB Grade WCC Grade WC1 Grade WC4 Grade WC5 Grade WC6 Grade WC9 Grade C12 Grade C5 Grade C12A Grade CA15 Grade C Grade D — Grade WPB Grade WPC Grade WP1 Grade WP11, Class 1 Grade WP12, Class 1 Grade WP11, Class 2 Grade WP11, Class 3 Grade WP12, Class 2 Grade WP22, Class 3 Grade WP22, Class 1 Grade WP5 Grade WP9 Grade WP91 Grade WPR (Continued)
8
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S41000 S42900 S41500 S40500 S40900 S41008 S44400 S43000 S43035 S30600 S30200 S30400 S30409 S30403 S30453 S30451 S30500 S31600 S31640 S31609 S31603 S31653 S31651 S31635 S31700 S31703 S31753 S32100 S32109 S34700 S34709 S34800 S34809 S38100 S30452 S31050 S30941 S30940 S30909 S30908 S31008 S31040 S30815
Plate Plate Plate Plate Plate Plate Plate Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240
6 6 6 7 7 7 7 7 7 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 2 4 1 1 1 2 2 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 2 2 2 2 2
Type 410 Type 429 Grade S41500 Type 405 Type 409 Type 410S Type 18-2 Type 430 Type 439 Type 18-15 Type 302 Type 304 Type 304H Type 304L Type 304LN Type 304N Type 305 Type 316 Type 316Cb Type 316H Type 316L Type 316LN Type 316N Type 316Ti Type 317 Type 317L Type 317LN Type 321 Type 321H Type 347 Type 347H Type 348 Type 348H Type XM-15 Type XM-21 Type 310 MoLN Type 309HCb Type 309Cb Type 309H Type 309S Type 310S Type 310Cb S30815 (Continued)
9
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S21800 S20100 S20200 S21600 S21603 S20910 S24000 S31726 S31725 S31254 S31200 S31260 S31803 S32101 S32205 S32750 S32760 S32550 S32950 S32900 S44635 S44627 S44626 S44700 S44800 S44660 K11510 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S30400 S30409 S30403 S30453 S30451 S31600
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate Plate Plate Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate Plate Shapes, Plates & Bars Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 242 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249
8 8 8 8 8 8 8 8 8 8 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10I 10I 10I 10J 10K 10K 1 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
3 3 3 3 3 3 3 4 4 4 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
S21800 Type 201-1 Type 202 Type XM-17 Type XM-18 Type XM-19 Type XM-29 Type 317LHM Type 317LM S31254 S31200 S31260 S31803 — S32205 — — Type 255 S32950 Type 329 S44635 Type XM-27 Type XM-33 Grade 29-4 S44800 S44660 Type 1 TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H TP348 TP348H Type 304 Type 304H Type 304L Type 304LN Type 304N Type 316 (Continued)
10
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 250 A 250 A 250 A 250 A 250 A 250 A 252 A 252 A 252 A 266 A 266 A 266 A 266 A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 268
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 3 3 3 3 4 5A 1 1 1 1 1 1 1 6 6 6 7 7 7 7 7 7 7
1 1 1 2 2 2 2 2 2 2 2 2 2 3 3 3 3 4 4 4 1 1 1 1 1 1 1 1 1 1 2 2 2 1 2 4 1 1 1 1 2 2 2
Type 316H Type 316L Type XM-15 S30815 TP309Cb TP309H TP309HCb TP309S TP310Cb TP310H TP310S Type 309 Type 310 MoLN TP201 TP202 TPXM-19 TPXM-29 317LH 317LM S31254 Grade T1 Grade T1a Grade T1b Grade T2 Grade T11 Grade T22 Grade 1 Grade 2 Grade 3 Grade 1 Grade 2 Grade 3 Grade 4 Type 410 Type 429 S41500 S40800 Type 405 Type 409 Type 430Ti Type 18Cr-2Mo Type 430 Type 439 (Continued)
11
S31609 S31603 S38100 S30815 S30940 S30909 S30941 S30908 S31040 S31009 S31008 S30900 S31050 S20100 S20200 S20910 S24000 S31726 S31725 S31254 K11522 K12023 K11422 K11547 K11597 K21590
K03506 K03506 K05001 K03017 S41000 S42900 S41500 S40800 S40500 S40900 S43036 S44400 S43000 S43035
Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube ERW Tube ERW Tube ERW Tube ERW Tube ERW Tube ERW Tube Pipe Piles Pipe Piles Pipe Piles Seamless Forging Seamless Forging Seamless Forging Seamless Forging Tube Tube Seamless & Welded Tube Seamless & Welded Tube Tube Tube Seamless & Welded Tube Seamless & Welded Tube Tube Seamless & Welded Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S44635 S44627 S44626 S44600 S44600 S44700 S44735 S44660 S44800 S30400 S30403 S31600 S31603 S30453 S31653 S31700 S32100 S34700 S34800 S21900 S21904 S38100 S20910 S24000 S30400 S30400 S30409 S31600 S31609 S32100 S32109 S34700 S34709 S41000 S30400 S30403 S31600 S31603 S32101 S32205 S32550 K01804 K02001
Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Tube Tube Tube Tube Tube Seamless & Welded Pipe Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Bar Bar Bar Bar Bar Bar & Shapes Bar & Shapes Bar & Shapes Plate Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 268 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 270 A 271 A 271 A 271 A 271 A 271 A 271 A 271 A 271 A 276 A 276 A 276 A 276 A 276 A 276 A 276 A 276 A 283 A 283
10I 10I 10I 10I 10I 10J 10J 10K 10K 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 6 8 8 8 8 10H 10H 10H 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 3 3 3 3 3 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Grade 25-4-4 TPXM-27 TPXM-33 Type 446-1 Type 446-2 Grade 29-4 S44735 Grade 26-3-3 Grade 29-4-2 TP304 TP304L TP316 TP316L Type 304LN Type 316LN Type 317 Type 321 Type 347 Type 348 Type XM-10 Type XM-11 Type XM-15 Type XM-19 Type XM-29 Type 304 Type 304 Type 304H Type 316 Type 316H Type 321 Type 321H Type 347 Type 347H Type 410 Type 304 Type 304L Type 316 Type 316L — — — Grade A Grade B (Continued)
12
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K02401 K02702 K01700 K02200 K02801 J93403 J92603 J93503 J94003 J94224 K02803 K12021 K12022 K12039 K12054 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32100 S32109 S32109 S34700 S34709 S34800 S34809 S38100 S30815 S30940 S30909 S30941 S30908 S31040 S31000
Plate Plate Plate Plate Plate Castings Castings Castings Castings Castings Plate Plate Plate & Sheet Plate & Sheet Plate & Sheet Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 283 A 283 A 285 A 285 A 285 A 297 A 297 A 297 A 297 A 297 A 299 A 302 A 302 A 302 A 302 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312
1 1 1 1 1 8 8 8 8 8 1 3 3 3 3 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 2 2 2 2 2 2 2 3 3 3 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 2 2 2 2
Grade C Grade D Grade A Grade B Grade C HE HF HH HI HK Grade A Grade A Grade B Grade C Grade D TP304 TP304H TP304L TP304LN TP304N TP316 TP316H TP316L TP316LN TP316N TP317 TP317L TP321 TP321 TP321H TP321H TP347 TP347H TP348 TP348H TPXM-15 S30815 TP309Cb TP309H TP309HCb TP309S TP310Cb TP310H (Continued)
13
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S31041 S31050 S31008 S20910 S21904 S24000 S31725 S31726 S31254 K03008 K03006 — K11267 K21903 K22035 K31918 K81340 K31918 K03008 K03006 K21903 K81340 K22035 K11522 K11578 K11547 K11597 K11562 K31545 K21590 K41545 K51545 K41245 S50400 K91560 K12520 K11597 K11572 K11572 K11564 K31545 K31545 K21590
Seamless & Welded Pipe Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Pipe Pipe Pipe Pipe Pipe Seamless & Welded Pipe Tube Welded Tube Welded Tube Tube Tube Tube Seamless Pipe Seamless Pipe Seamless Pipe Pipe Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Forging Forging Forging Forging Forging Forging Forging Forging
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 333 A 333 A 333 A 333 A 333 A 333 A 333 A 333 A 334 A 334 A 334 A 334 A 334 A 334 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 335 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336
8 8 8 8 8 8 8 8 8 1 1 1 4 9A 9A 9B 11A 9B 1 1 9A 11A 9A 3 3 3 4 4 5A 5A 5B 5B 5B 5B 5B 3 4 4 4 4 5A 5A 5A
2 2 2 3 3 3 4 4 4 1 1 3 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 1 1 1 1 1 1 1
TP310HCb TP310MoLN TP310S TPXM-19 TP-11 TPXM-29 317LM 317LM S31254 Grade 1 Grade 6 Grade 10 Grade 4 Grade 7 Grade 9 Grade 3 Grade 8 Grade 3 Grade 1 Grade 6 Grade 7 Grade 8 Grade 9 Grade P1 Grade P15 Grade P2 Grade P11 Grade P12 Grade P21 Grade P22 Grade P5 Grade P5b Grade P5c Grade P9 Grade P91 Grade F1 Grade F11, Class 1 Grade F11, Class 2 Grade F11, Class 3 Grade F12 Grade F21, Class 1 Grade F21, Class 3 Grade F22, Class 1 (Continued)
14
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K21590 K41545 K42544 K90941 K90901 K31830 S41000 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S32109 S34700 S34709 S34800 S34809 S31000 S21904 S20910 S30600 S44627 K03009 — K03011 K12202 K12202 K12202 — K13050 K13050 K22036 K32025 J92590 J92901 — J92500
Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Castings Castings Castings Castings
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 350 A 350 A 350 A 350 A 350 A 350 A 350 A 350 A 350 A 350 A 350 A 351 A 351 A 351 A 351
5A 5B 5B 5B 5B 5C 6 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 10I 1 1 1 1 1 1 1 9A 9A 9A 9B 8 8 8 8
1 1 1 1 2 1 3 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 3 3 4 1 1 2 2 2 3 3 3 1 1 1 1 1 1 1 1
Grade F22, Class 3 Grade F5 Grade F5A Grade F9 Grade F91 Grade F3V Grade F6 F304 F304H F304L F304LN F304N F316 F316H F316L F316LN F316N F321 F321H F347 F347H F348 F348H F310 FXM-11 FXM-19 F46 Grade FXM-27Cb Grade LF1 Grade LF787, Class 2 Grade LF2 Grade LF6 Grade LF6, Class 2 Grade LF6, Class 3 Grade LF787, Class 3 Grade LF5, Class 1 Grade LF5, Class 2 Grade LF9 Grade LF3, Class 2 CF10 CF10M CF10MC CF3 (Continued)
15
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
J92500 J92800 J92600 J92600 J92710 J92900 J93000 J92802 J93401 J93402 J93400 J94202 J94204 J93790 J93370 J93380 — J12522 J02504 J03003 J02505 J91540 J22500 J31550 J41500 J42215 K81340 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S34700 S34800 S30815 S30900 S30940
Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Plate Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 352 A 352 A 352 A 352 A 352 A 352 A 352 A 352 A 352 A 353 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358
8 8 8 8 8 8 8 8 8 8 8 8 8 8 10H 10H 10H 3 1 1 1 6 9A 9B 9C 11A 11A 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 2 2 2 2 2 2 3 1 1 1 1 1 1 2 4 1 1 1 5 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2
CF3A CF3M CF8 CF8A CF8C CF8M CG8M CE20N CH10 CH20 CH8 CK20 HK40 CG6MMN CD4MCu CD3MWCuN CE8MN Grade LC1 Grade LCA Grade LCB Grade LCC Grade CA6NM Grade LC2 Grade LC3 Grade LC4 Grade LC2-1 — 304 304H 304L 304LN 304N 316 316H 316L 316LN 316N 321 347 348 253MA 309 309Cb (Continued)
16
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S30908 S31000 S31040 S31008 S20910 S24000 S31726 S31725 S31254 — K02501 K03006 K11522 K11547 K11597 K11562 K31545 K21590 K41545 K90941 S50460 K03002 K04001 S16800 S30400 S30409 S30453 S30451 S31600 S31609 S31653 S31651 S32100 S32109 S34700 S34709 S34800 S31726 S31725 K03013 — — —
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Sheet Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forging Forging Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Tube Seamless Tube Pipe Pipe Pipe Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 366 A 369 A 369 A 369 A 369 A 369 A 369 A 369 A 369 A 369 A 369 A 369 A 372 A 372 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 381 A 381 A 381 A 381
8 8 8 8 8 8 8 8 8 1 1 1 3 3 4 4 5A 5A 5B 5B 5B 1 1 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 1 1 1 1
2 2 2 2 3 3 4 4 4 1 1 1 1 1 1 1 1 1 1 1 2 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 4 4 1 1 1 1
309S 310 310Cb 310S XM-19 XM-29 317L4 317LM S31254 Commercial Quality Grade FPA Grade FPB Grade FP1 Grade FP2 Grade FP11 Grade FP12 Grade FP21 Grade FP22 Grade FP5 Grade FP9 Grade FP91 Grade A Grade B 16-8-2H TP304 TP304H TP304LN TP304N TP316 TP316H TP316LN TP316N TP321 TP321H TP347 TP347H TP348 317L4 317LM Class Y35 Class Y42 Class Y46 Class Y48 (Continued)
17
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
— — — K12143 K12143 K11789 K11789 K11757 K11757 K31545 K31545 K21590 K21590 K41545 K41545 S50460 J12080 J12092 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S30900 S31000 S20910 K11591 S30400 S30403 S31600
Pipe Pipe Pipe Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Castings Castings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Cast Pipe Welded Pipe Welded Pipe Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 381 A 381 A 381 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 387 A 389 A 389 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 405 A 409 A 409 A 409
1 1 1 3 3 4 4 4 4 5A 5A 5A 5A 5B 5B 5B 4 4 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 4 8 8 8
2 2 2 1 2 1 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 3 1 1 1 1
Class Y50 Class Y52 Class Y56 Grade 2, Class 1 Grade 2, Class 2 Grade 11, Class 1 Grade 11, Class 2 Grade 12, Class 1 Grade 12, Class 2 Grade 21, Class 1 Grade 21, Class 2 Grade 22, Class 1 Grade 22, Class 2 Grade 5, Class 1 Grade 5, Class 2 Grade 91, Class 2 Grade C23 Grade C24 WP304 WP304H WP304L WP304LN WP304N WP316 WP316H WP316L WP316LN WP316N WP317 WP317L WP321 WP321H WP347 WP347H WP348 WP348H WP309 WP310 WPXM-19 Grade P24 TP304 TP304L TP316 (Continued)
18
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S31603 S31700 S32100 S34700 S34800 S30815 S30940 S31726 S31725 S31254 K01501 K02201 K02503 K02505 K02704 K03102 K03103 — K22035 — K81340 K11535 K11540 J12521 J11522 J11547 J12072 J11562 J31545 J21890 J42045 J51545 J82090 J91150 S16800 S30400 S30409 S30451 S31600 S31609 S31651 S32100 S32109
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Sheet Sheet Sheet Sheet Sheet Sheet Sheet Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Tube Tube Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 414 A 414 A 414 A 414 A 414 A 414 A 414 A 420 A 420 A 420 A 420 A 423 A 423 A 426 A 426 A 426 A 426 A 426 A 426 A 426 A 426 A 426 A 426 A 426 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430
8 8 8 8 8 8 8 8 8 8 1 1 1 1 1 1 1 1 9A 9B 11A 4 4 3 3 3 4 4 5A 5A 5B 5B 5B 6 8 8 8 8 8 8 8 8 8
1 1 1 1 1 2 2 4 4 4 1 1 1 1 1 2 2 1 1 1 1 2 2 1 1 1 1 1 1 1 1 1 1 3 1 1 1 1 1 1 1 1 1
TP316L TP317 TP321 TP347 TP348 253MA TP309Cb 317L4 317LM S31254 Grade A Grade B Grade C Grade D Grade E Grade F Grade G Grade WPL6 Grade WPL9 Grade WPL3 Grade WPL8 Grade 1 Grade 2 Grade CP1 Grade CP15 Grade CP2 Grade CP11 Grade CP12 Grade CP21 Grade CP22 Grade CP5 Grade CP5b Grade CP9 Grade CPCA15 FP16-8-2H FP304 FP304H FP304N FP316 FP316H FP316N FP321 FP321H (Continued)
19
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S34700 S34709 J92971 J92500 J92500 J92800 J92600 J92600 J92710 J92900 S30409 S31609 S34709 K03300 S30200 S30215 S30300 S30323 S30400 S30403 S30500 S31600 S31603 S31700 S32100 S34700 S34800 S40300 S41000 S41400 S30800 S31400 S40500 S42000 S42900 S43000 S20200 S21900 S21904 S40300 S41000 S41400 S41500
Forged Pipe Forged Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Plate Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 430 A 430 A 451 A 451 A 451 A 451 A 451 A 451 A 451 A 451 A 452 A 452 A 452 A 455 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 479 A 479 A 479 A 479
8 8 8 8 8 8 8 8 8 8 8 8 8 1 8 8 8 8 8 8 8 8 8 8 8 8 8 6 6 6 8 8 6 6 6 6 8 8 8 6 6 6 6
1 1 1 1 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 2 2 2 3 3 3 1 1 3 4
FP347 FP347H CPF10MC CPF3 CPF3A CPF3M CPF8 CPF8A CPF8C CPF8M TP304H TP316H TP347H — Type 302 Type 302B Type 303 Type 303Se Type 304 Type 304L Type 305 Type 316 Type 316L Type 317 Type 321 Type 347 Type 348 Type 403 Type 410 Type 414 Type 308 Type 314 Type 405 Type 420 Type 429 Type 430 Type 202 Type XM-10 Type XM-11 Type 403 Type 410 Type 414 S41500 (Continued)
20
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S40500 S44400 S43000 S43035 S41040 S30409 S30403 S30453 S30451 S31640 S31609 S31603 S31653 S31651 S31635 S32109 S34709 S34809 S30600 S30200 S30400 S31600 S32100 S34700 S34800 S21800 S21904 S21600 S21603 S20910 S24000 S31726 S31725 S31254 S32550 S31803 S32101 S32205 S32550 S44627 S44700 S44800 J31200
Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Castings
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 487
7 7 7 7 7 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 10H 10H 10H 10H 10H 10I 10J 10K 1
1 2 2 2 3 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 3 3 3 3 3 3 4 4 4 1 1 1 1 1 1 1 1 2
Type 405 Type 444 Type 430 Type 439 Type XM-30 304H 304L 304LN 304N 316Cb 316H 316L 316LN 316N 316Ti 321H 347H 348H 306 Type 302 Type 304 Type 316 Type 321 Type 347 Type 348 S21800 XM-11 XM-17 XM-18 XM-19 XM-29 317L4 317LM S31254 F255 — — — — Type XM-27 Grade 28-4 Grade 28-4-2 Grade 16, Class A (Continued)
21
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
J13047 J22091 J22091 J22091 J91450 J91171 J91171 J91451 J91540 J91540 J13002 J13002 J13002 J13005 J13005 J13047 J13047 J13047 K03000 K03000 K02705 K03000 K13502 K13502 K12766 K12766 K12042 K12042 K22375 K31830 K22375 K22375 K42365 K42365 G10100 G10150 G10180 G10200 G10250 G11170 G10100 G10150 G10200
Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Tube Tube Tube Tube Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 487 A 500 A 500 A 500 A 501 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 508 A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 512
3 5C 5C 5C 6 6 6 6 6 6 10A 10A 10A 10F 10F 10F 11A 11A 1 1 1 1 1 1 3 3 3 3 3 5C 11A 11A 11A 11A 1 1 1 1 1 1 1 1 1
3 1 4 4 3 3 3 3 4 4 1 1 1 1 1 1 3 3 1 1 1 1 2 2 3 3 3 3 3 1 5 5 5 5 1 1 1 1 1 1 1 1 1
Grade 4, Class C Grade 8, Class A Grade 8, Class B Grade 8, Class C Grade CA15, Class B Grade CA15, Class C Grade CA15, Class D Grade CA15M, Class A Grade CA6NM, Class A Grade CA6NM, Class B Grade 1, Class A Grade 1, Class B Grade Mn-V Grade 2, Class A Grade 2, Class B Grade 4, Class A Grade 4, Class B Grade 4, Class E Grade A Grade B Grade C — Grade 1 Grade 1A Grade 2, Class 1 Grade 2, Class 2 Grade 3, Class 1 Grade 3, Class 2 Grade 4N, Class 3 Grade 3V Grade 4N, Class 1 Grade 4N, Class 2 Grade 5, Class 1 Grade 5, Class 2 Grade 1010 Grade 1015 Grade 1018 Grade 1020 Grade 1025 Grade 1117 Grade MT1010 Grade MT1015 Grade MT1020 (Continued)
22
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
— — G10300 G10080 G10100 G10150 G10150 G10170 G10180 G10190 G10200 G10210 G10250 G10110 G10150 G10200 — — G10200 G10250 G10260 G10300 K11856 K11856 K11576 K21604 K11576 K11511 K11625 K11523 — — K21650 — — — K02001 K02401 K02800 K03101 K01800 K02100 K02403
Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Plate Plate Plate & Shapes Plate & Shapes Plate Plate & Shapes Plate & Shapes Plate & Shapes Plate Plate & Shapes Plate & Shapes Plate Plate & Shapes Plate & Shapes Plate Plate Plate Plate Plate Plate Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 512 A 512 A 512 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 515 A 515 A 515 A 515 A 516 A 516 A 516
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 1 1 1 1 1 1 1
1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 2 1 2 3 3 4 6 6 6 6 6 8 9 10 12 1 1 1 2 1 1 1
Grade MTX1015 Grade MTX1020 Grade 1030 Grade 1008 Grade 1010 Grade 1015 Grade 1015 CW Grade 1017 Grade 1018 Grade 1019 Grade 1020 Grade 1021 Grade 1025 Grade MT1010 Grade MT1015 Grade MT1020 Grade MTX1015 Grade MTX1020 Grade 1020 CW Grade 1025 CW Grade 1026 Grade 1030 Grade A Grade E Grade F Grade H Grade B Grade C Grade J Grade K Grade S Grade T Grade P Grade Q Grade M Grade R Grade 55 Grade 60 Grade 65 Grade 70 Grade 55 Grade 60 Grade 65 (Continued)
23
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K02700 K11856 K21604 K11576 K21604 K11630 K11625 K11523 — — K21650 — K11683 G10080 G10120 G10160 G10170 G10180 G10180 G10190 G10200 G10200 G10210 G10220 G10220 G10250 G10250 G10260 G10260 G10100 G10150 G10200 G10150 G10300 G41300 G86300 — — — K81340 K71340 KO2504 KO3005
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Die Forging Die Forging Forging Forging Forging Pipe Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 516 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 517 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 521 A 521 A 521 A 522 A 522 A 523 A 523
1 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 11B 11B 1 1 1 11A 11A 1 1
2 1 2 3 3 4 6 6 6 6 8 9 10 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 9 9 1 1 2 1 1 1 1
Grade 70 Grade A Grade E Grade F Grade H Grade B Grade J Grade K Grade S Grade T Grade P Grade Q Grade M Grade 1008 Grade 1012 Grade 1016 Grade 1017 Grade 1018 Grade 1018 HR Grade 1019 Grade 1020 Grade 1020 HR Grade 1021 Grade 1022 Grade 1022 HR Grade 1025 Grade 1025 HR Grade 1026 Grade 1026 HR Grade MT1010 Grade MT1015 Grade MT1020 Grade MTX1015 Grade 1030 Grade 4130 Grade 8630 Class CC Class CCI Class CE Type I Type II Grade A Grade B (Continued)
24
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
KO2104 KO2104 KO2104 KO2104 KO2703 — — K12521 K12521 K12539 K12539 K12554 K12554 K12529 K12529 K12521 K12539 K12554 K12529 K02400 K02400 K02400 K01506 K03506 — K12765 K12765 K12045 K12045 K11572 K21390 K31830 K21390 K21390 K21590 K21590 K21590 K21590 K31830 K31830 K31835 K21590 K21590
Pipe Pipe Galvanized Sheet Galvanized Sheet Structural Bar, Plate & Shapes Bar, Plate & Shapes Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Coiled Tube Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 524 A 524 A 526 A 527 A 529 A 529 A 529 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 537 A 537 A 537 A 539 A 541 A 541 A 541 A 541 A 541 A 541 A 541 A 541 A 541 A 541 A 541 A 542 A 542 A 542 A 542 A 542 A 542 A 542 A 542 A 542
1 1 1 1 1 1 1 3 3 3 3 3 3 3 3 11A 11A 11A 11A 1 1 1 1 1 1 3 3 3 3 4 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C
1 1 1 1 1 2 2 3 3 3 3 3 3 3 3 4 4 4 4 2 3 3 1 2 2 3 3 3 3 1 1 1 4 5 1 1 1 1 1 1 1 3 3
Grade I Grade II Grade II Grade II Grade 42 Grade 50 Grade 55 Type A, Class 1 Type A, Class 2 Type B, Class 1 Type B, Class 2 Type C, Class 1 Type C, Class 2 Type D, Class 1 Type D, Class 2 Grade A, Class 3 Grade B, Class 3 Grade C, Class 3 Grade D, Class 3 Class 1 Class 2 Class 3 — Grade 1 Grade 1A Grade 2, Class 1 Grade 2, Class 2 Grade 3, Class 1 Grade 3, Class 2 Grade 11, Class 4 Grade 22, Class 3 Grade 3V Grade 22, Class 4 Grade 22, Class 5 Type A, Class 4 Type A, Class 4a Type B, Class 4 Type B, Class 4a Type C, Class 4 Type C, Class 4a Type D, Class 4a Type A, Class 3 Type B, Class 3 (Continued)
25
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K31830 K21590 K21590 K31830 K21590 K21590 K31830 K42339 K42338 K42339 K42339 K42338 K42338 K81340 K71340 K01807 K02707 K03006 K01807 K03007 K03505 K11224 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02303 K02304 — K02305 K02306 K02301 K02404 K02701
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Seamless Tube Seamless Tube Seamless Tube Tube-RW Tube-RW ERW Tube Plate Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Shapes, Plate & Bars Shapes, Plate & Bars Plate & Shapes Plate & Bars Shapes Plate Plate Improved Toughness Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 542 A 542 A 542 A 542 A 542 A 542 A 542 A 543 A 543 A 543 A 543 A 543 A 543 A 553 A 553 A 556 A 556 A 556 A 557 A 557 A 557 A 562 A 569 A 569 A 569 A 569 A 569 A 569 A 570 A 570 A 570 A 570 A 570 A 570 A 570 A 572 A 572 A 572 A 572 A 572 A 573 A 573 A 573
5C 5C 5C 5C 5C 5C 5C 11B 11B 11A 11A 11A 11A 11A 11A 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
3 4 4 4 5 5 5 10 10 5 5 5 5 1 1 1 1 2 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 3 3 1 1 2
Type C, Class 3 Type A, Class 1 Type B, Class 1 Type C, Class 1 Type A, Class 2 Type B, Class 2 Type C, Class 2 Type B, Class 2 Type C, Class 2 Type B, Class 1 Type B, Class 3 Type C, Class 1 Type C, Class 3 Type I Type II Grade A2 Grade B2 Grade C2 Grade A2 Grade B2 Grade C2 — Grade 30 Grade 33 Grade 36 Grade 40 Grade 45 Grade 50 Grade 30 Grade 33 Grade 36 Grade 40 Grade 45 Grade 50 Grade 55 Grade 42 Grade 50 Grade 55 Grade 60 Grade 65 Grade 58 Grade 65 Grade 70 (Continued)
26
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
G10080 G10100 G10120 G10150 G10170 G10200 G10230 G10250 G10080 G10100 G10120 G10150 G10160 G10170 G10180 G10190 G10200 G10210 G10220 G10230 G10250 K11500 K01807 K03007 — K11430 K12043 K11538 — K11856 K11695 K11576 K02004 K02005 K11526 — — — — — — — —
Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Pipe Tube-RW Tube-RW Structural Shapes Plate & Bars Plate & Bars Plate & Bars Plate & Bars Forging Forging Forging Tapered Tube Tapered Tube Tapered Tube Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 575 A 575 A 575 A 575 A 575 A 575 A 575 A 575 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 587 A 587 A 587 A 588 A 588 A 588 A 588 A 588 A 592 A 592 A 592 A 595 A 595 A 595 A 606 A 606 A 607 A 607 A 607 A 607 A 607 A 607
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 11B 11B 11B 1 1 3 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 2 2 2 2 1 2 3 2 2 1 2 2 1 1 2 3 3 3
Grade M1008 Grade M1010 Grade M1012 Grade M1015 Grade M1017 Grade M1020 Grade M1023 Grade M1025 Grade 1008 Grade 1010 Grade 1012 Grade 1015 Grade 1016 Grade 1017 Grade 1018 Grade 1019 Grade 1020 Grade 1021 Grade 1022 Grade 1023 Grade 1025 — Grade A2 Grade B2 All Grades Grade A Grade B Grade C Grade K Grade A Grade E Grade F Grade A Grade B Grade C Type 2 Type 4 Grade 45 Grade 50 Grade 55 Grade 60 Grade 65 Grade 70 (Continued)
27
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
G10170 G10170 G10170 G10120 G10170 K02900 — — K12700 — K02601 K12609 K00040 K00040 K01802 K12000 K12037 K12202 K41583 — — — — K11804 K11804 K11804 K11804 J02504 J03003 J02505 K01701 K02203 K02007 — — — — — — — — — S30200
Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Plate Rebar Rebar Tube HSLA Tube HSLA Tube Tube Sheet Sheet Plate & Shapes HSLA Steel HSLA Steel HSLA Steel Plate Galvanized Sheet Galvanized Sheet Galvanized Sheet Galvanized Sheet Hi-Str. Lo-Alloy Plate Hi-Str. Lo-Alloy Plate Hi-Str. Lo-Alloy Plate Hi-Str. Lo-Alloy Plate Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Plate Plate Plate Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Bar, Shapes, Rounds, Squares, Hex. Flat Bar Bar, Shapes, Rounds, Squares, Hex. Plate, Sheet & Strip
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 611 A 611 A 611 A 611 A 611 A 612 A 615 A 615 A 618 A 618 A 618 A 618 A 620 A 620 A 633 A 633 A 633 A 633 A 645 A 653 A 653 A 653 A 653 A 656 A 656 A 656 A 656 A 660 A 660 A 660 A 662 A 662 A 662 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 666
1 1 1 1 1 10C 1A 1A 1 1 1 1 1 1 1 1 1 1 11A 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 8
1 1 1 1 3 1 4 4 1 2 2 2 1 1 1 2 2 3 2 1 1 1 1 1 1 2 3 1 2 2 1 1 2 1 1 1 1 1 3 3 3 3 1
Grade A Grade B Grade C Grade D Grade E — Grade 40 Grade 60 Grade III Grade 1a Grade 1b Grade II Types A Types B Grade A Grade C Grade D Grade E — Grade 33 Grade 37 Grade 40 Grade 80 Grade 50 Grade 60 Grade 70 Grade 80 Grade WCA Grade WCB Grade WCC Grade A Grade B Grade C Grade 45 Grade 50 Grade 55 Grade 60 Grade 65 Grade 70 Grade 75 Grade 79 Grade 80 Type 302 (Continued)
28
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S30400 S30403 S30453 S30451 S31600 S31603 S31651 S20100 S21904 G10200 G10250 G10300 — K02801 K02401 K02800 K02100 K02403 K03101 K02700 K02400 K02803 K02400 K01700 K02200 K02801 K02401 K02800 K01800 K02100 K02403 K02402 K11820 K03101 K02700 K02400 K12021 K12020 K12320 K02803 K02400 K12022 K12554
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Forging Forging Forging Forging Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 666 A 666 A 666 A 666 A 666 A 666 A 666 A 666 A 666 A 668 A 668 A 668 A 668 A 671 A 671 A 671 A 671 A 671 A 671 A 671 A 671 A 671 A 671 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672 A 672
8 8 8 8 8 8 8 8 8 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 3 1 1 1 3 3 3 1 1 3 3
1 1 1 1 1 1 1 3 3 1 1 2 3 1 1 1 1 1 2 2 2 2 3 1 1 1 1 1 1 1 1 1 1 2 2 2 2 2 2 2 3 3 3
Type 304 Type 304L Type 304LN Type 304N Type 316 Type 316L Type 316N 201 XM-11 Class B Class C Class D Class F Grade CA55 Grade CB60 Grade CB65 Grade CC60 Grade CC65 Grade CB70 Grade CC70 Grade CD70 Grade CK75 Grade CD80 Grade A45 Grade A50 Grade A55 Grade B60 Grade B65 Grade C55 Grade C60 Grade C65 Grade E60 Grade L65 Grade B70 Grade C70 Grade D70 Grade H75 Grade L70 Grade L75 Grade N75 Grade D80 Grade H80 Grade J80 (Continued)
29
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K12554 K12521 — — — — — — — K01600 K02002 K02204 K02204 K02204 K12202 S30400 S30403 S30453 S30451 S31600 S31603 S31653 S31651 S24000 K12249 K02803 K02400 K02400 K12143 K11820 K12143 K12020 K12320 K11757 K11789 K11757 K11789 K21590 K21590 K31545 K31545 K41545 K41545
Fusion Welded Pipe Fusion Welded Pipe Bar Bar Bar Bar Bar Bar Bar Structural Plate Structural Plate Structural Plate Structural Plate Structural Plate Structural Plate Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Marine Piling—Plate & Bar Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 672 A 672 A 675 A 675 A 675 A 675 A 675 A 675 A 675 A 678 A 678 A 678 A 678 A 678 A 678 A 688 A 688 A 688 A 688 A 688 A 688 A 688 A 688 A 688 A 690 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691 A 691
3 11A 1 1 1 1 1 1 1 1 1 1 1 1 1 8 8 8 8 8 8 8 8 8 1 1 1 1 3 3 3 3 3 4 4 4 4 5A 5A 5A 5A 5B 5B
3 4 1 1 1 1 1 2 2 2 2 3 3 3 3 1 1 1 1 1 1 1 1 3 2 2 2 3 1 1 2 2 2 1 1 1 1 1 1 1 1 1 1
Grade J90 Grade J100 Grade 45 Grade 50 Grade 55 Grade 60 Grade 65 Grade 70 Grade 75 Grade A Grade B Grade C Grade C Grade C Grade D TP304 TP304L TP304LN TP304N TP316 TP316L TP316LN TP316N TPXM-29 — Grade CMS-75 Grade CMSH-70 Grade CMSH-80 Grade 1/2 CR, Class 1 Grade CM-65, Gr. A Grade 1/2 CR, Class 2 Grade CM-70 Grade CM-75 Grade 1.25CR, Class 1 Grade 1.25CR, Class 2 Grade 1CR, Class 1 Grade 1CR, Class 2 Grade 2-1/4CR, Class 1 Grade 2-1/4CR, Class 2 Grade 3CR, Class 1 Grade 3CR, Class 2 Grade 5CR, Class 1 Grade 5CR, Class 2 (Continued)
30
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
K03504 K03504 K03200 K03200 K03011 K02302 K03301 K12510 K12089 K20934 K02302 K03301 K12510 K12089 K12089 K20934 K03301 K12510 K20934 K20934 K02902 K02902 K02902 K02902 K32218 K32218 K42247 K42247 K42247 K42247 — — — K11856 K11856 K21604 K21604 K11576 K11576 K21504 K21504 K11630 K11630
Bar Bar Bar Bar Rebar Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Plate, Bars & Shapes Plate, Bars & Shapes Plate, Bars & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 695 A 695 A 696 A 696 A 706 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 707 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709
1 1 1 1 1A 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 3 3 3 3 9B 9B 11A 11A 11A 11A 1 1 1 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B
1 2 1 2 4 1 1 1 1 1 2 2 2 2 2 2 3 3 3 4 1 2 3 4 1 1 1 2 3 4 1 1 2 1 1 2 2 3 3 3 3 4 4
Type B Type B, Grade 40 Grade B Grade C — Grade L1, Class 1 Grade L2, Class 1 Grade L3, Class 1 Grade L4, Class 1 Grade L5, Class 1 Grade L1, Class 2 Grade L2, Class 2 Grade L3, Class 2 Grade L4, Class 2 Grade L4, Class 3 Grade L5, Class 2 Grade L2, Class 3 Grade L3, Class 3 Grade L5, Class 3 Grade L5, Class 4 Grade L6, Class 1 Grade L6, Class 2 Grade L6, Class 3 Grade L6, Class 4 Grade L7, Class 1 Grade L7, Class 2 Grade L8, Class 1 Grade L8, Class 2 Grade L8, Class 3 Grade L8, Class 4 Grade 36 Grade 50 Grade 50W Grade 100, Type A Grade 100W, Type A Grade 100, Type E Grade 100W, Type E Grade 100, Type F Grade 100W, Type F Grade 100, Type H Grade 100W, Type H Grade 100, Type B Grade 100W, Type B (Continued)
31
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
— — K11625 K11625 K21650 K21650 — — — — — K20747 K20747 K20747 K22035 K11831 K12031 K12037 K02506 S41500 S43035 S44400 S44627 S44626 S44700 S44660 S44800 K21205 K12001 K12202 K12447 K12447 — K11797 K21390 J91150 J91151 J92615 J93423 J92500 J92600 J92710 J92900
Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Structural Structural Structural Welded Pipe Plate Plate Plate Forging Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Pressure Vessel Plate Plate Plate Plate Plate Plate Bar Bar Castings Castings Castings Castings Castings Castings Castings Castings
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ;ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 709 A 710 A 710 A 710 A 714 A 724 A 724 A 724 A 727 A 731 A 731 A 731 A 731 A 731 A 731 A 731 A 731 A 734 A 737 A 737 A 738 A 738 A 738 A 739 A 739 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743
11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 11B 12A 12B 12C 9A 1 1 1 1 6 7 7 10I 10I 10J 10K 10K 11A 1 1 1 1 1 4 5A 6 6 8 8 8 8 8 8
6 6 6 6 8 8 9 9 10 10 11 1 1 1 1 4 4 4 1 4 2 2 1 1 1 1 1 2 2 3 2 3 3 1 1 3 3 1 1 1 1 1 1
Grade 100, Type C Grade 100W, Type C Grade 100, Type J Grade 100W, Type J Grade 100, Type P Grade 100W, Type P Grade 100, Type Q Grade 100W, Type Q Grade 100, Type M Grade 100W, Type M Grade HPS70W Grade A, Class 2 Grade A, Class 3 Grade A, Class 1 Grade V, Type E Grade A Grade B Grade C Grade 36 S41500 Type 439 Type 18Cr-2Mo TPXM-27 TPXM-33 S44700 Grade 26-3-3 Grade 29-4-2 Type A Grade B Grade C Grade A Grade B Grade C Grade B11 Grade B22 CA-15 CA-15M CC-50 CE-30 CF-3 CF-8 CF-8C CF-8M (Continued)
32
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
J92701 J92602 J93000 J93001 J93402 J91153 J91804 J92800 J92804 J92972 J93254 J92999 J94652 J91540 J93401 K03046 K03047 K03046 K32026 S30403 S31603 S31703 S32100 S34700 S30403 S31603 S31703 S32100 S34700 — — — S32304 S32550 S32950 S31803 S32750 S32900 S31200 S31260 S31500 S32101 S32205
Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Forging Forging Forging Forging As-Welded Wrought Fittings As-Welded Wrought Fittings As-Welded Wrought Fittings As-Welded Wrought Fittings As-Welded Wrought Fittings Welded Unannealed Tube Welded Unannealed Tube Welded Unannealed Tube Welded Unannealed Tube Welded Unannealed Tube Pressure Vessel Plate Pressure Vessel Plate Pressure Vessel Plate Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Tubing Tubing
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 765 A 765 A 765 A 765 A 774 A 774 A 774 A 774 A 774 A 778 A 778 A 778 A 778 A 778 A 782 A 782 A 782 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789
8 8 8 8 8 6 6 8 8 8 8 8 8 6 8 1 1 1 9B 8 8 8 8 8 8 8 8 8 8 11B 11B 11B 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H
1 2 1 1 2 4 4 1 1 1 4 1 1 4 2 1 2 3 1 1 1 1 1 1 1 1 1 1 1 4 4 4 1 1 1 1 1 1 1 1 1 1 1
CF-16F CF-20 CG-8M CG-12 CH-20 CA-40 CB-6 CF-3M CF-3MN CF-10SMnN CK-3MCuN CG-3M CN-3M CA-6NM CH-10 Grade I Grade II Grade IV Grade III TP304L TP316L TP317L TP321 TP347 TP304L TP316L TP317L TP321 TP347 Class 1 Class 2 Class 3 Grade 2304 Grade 2550 Grade 2950 S31803 S32750 S32900 S31200 S31260 S31500 — — (Continued)
33
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S32550 S32760 S31200 S31260 S31500 S31803 S32101 S32205 S32550 S32760 S32304 S32550 S32750 S32900 S32950 S32900 — — — — — S43035 S44660 K11852 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S38100
Tubing Tubing Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Tube Resistance Welded Pipe Resistance Welded Pipe Seamless Pipe Seamless Pipe Furnace-Welded Pipe Welded Tube Welded Tube Structural Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 789 A 789 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 795 A 795 A 795 A 795 A 795 A 803 A 803 A 808 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813
10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 1 1 1 1 1 7 10K 1 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
— — S31200 S31260 S31500 S31803 — — — — S32304 S32550 S32750 S32900 S32950 S32900 Type E, Grade A 1 Type, Grade B Type S, Grade A Type S, Grade B Type F Type 439 Grade 26-3-3 — TP304 TP304H TP304L TP304LN TP304N TP316 TP316H TP316L TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H TP348 TP348H TPXM-15 (Continued)
34
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
S21904 S20910 S24000 S31254 S31254 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S38100 S21904 S20910 S24000 S41500 S31803 S32205 S32550 S32760 G10060 G10080 G10090 G10100 G10120 G10150 G10160 G10170 G10180 G10190 G10200
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Pipe Fittings Wrought Pipe Fittings Wrought Pipe Fittings Wrought Pipe Fittings Wrought Pipe Fittings Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 813 A 813 A 813 A 813 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 815 A 815 A 815 A 815 A 815 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 6 10H 10H 10H 10H 1 1 1 1 1 1 1 1 1 1 1
3 3 3 4 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 3 3 3 4 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
TPXM-11 TPXM-19 TPXM-29 S31254 S31254 TP304 TP304H TP304L TP304LN TP304N TP316 TP316H TP316L TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H TP348 TP348H TPXM-15 TPXM-11 TPXM-19 TPXM-29 S41500 S31803 S32205 S32550 S32760 1006 1008 1009 1010 1012 1015 1016 1017 1018 1019 1020 (Continued)
35
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
G10210 G10220 G10230 G10250 K31830 K31835 — — K81340 K12043 — — — — — — J93370 J93372 J93373 J93345 J93371 J92205 J93404 J93380 — — — — S32205 S32550 S32760 — — — — — — — — — — — —
Plate Plate Plate Plate Plate Pressure Vessel Plate Forging Plate Pressure Vessel Plate Plate & Shapes Sheet Piling Sheet Piling Sheet Piling Sheet Piling Plate & Shapes Plate & Shapes Casting Casting Casting Casting Casting Casting Casting Casting Structural Structural Shapes Structural Shapes Structural Shapes Welded Pipe Welded Pipe Welded Pipe Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 830 A 830 A 830 A 830 A 832 A 832 A 836 A 841 A 844 A 852 A 857 A 857 A 857 A 857 A 871 A 871 A 890 A 890 A 890 A 890 A 890 A 890 A 890 A 890 A 913 A 913 A 913 A 913 A 928 A 928 A 928 A 935 A 935 A 935 A 935 A 935 A 935 A 935 A 935 A 935 A 935 A 935 A 935
1 1 1 1 5C 5C 1 10C 11A 11B 1 1 1 1 3 3 10H 10H 10H 10H 10H 10H 10H 10H 1 1 1 1 10H 10H 10H 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 11 1 1 1 1 2 3 1 1 1 1 1 1 1 1 2 3 3 4 1 1 1 1 1 1 1 2 2 2 2 3 3 3 4
1021 1022 1023 1025 Grade 21V Grade 22V Class 1 TMCP, Class 1 Grade 9% Ni Grade 70W Grade 25 Grade 30 Grade 33 Grade 36 Grade 60 Grade 65 1A 1B 1C 2A 3A 4A 5A 6A Grade 50 Grade 60 Grade 65 Grade 70 2205 255 — Grade 45, Class 1 Grade 45, Class 2 Grade 50, Class 1 Grade 50, Class 2 Grade 55, Class 1 Grade 55, Class 2 Grade 60, Class 1 Grade 60, Class 2 Grade 65, Class 1 Grade 65, Class 2 Grade 70, Class 2 Grade 70, Class 1 (Continued)
36
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 945 A 945 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 984 A 984 A 984 A 984 A 984 A 992 A 995 A 995 A 995 A 995 A 995 A 995 A 1008 A 1008 A 1008 A 1008 A 1008 A 1008 A 1008 A 1008 A 1008
3 3 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 1 1 1 1 1 1 10H 10H 10H 10H 10H 10H 1 1 1 1 1 1 1 1 1
1 2 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 2 3 3 4 1 2 2 2 4 1 1 1 1 1 1 1 1 1 1 1 1 1 3 4 3
Grade 50 Grade 65 F304 F304H F304L F304LN F304N F316 F316H F316L F316LN F316N F321 F321H F347 F347H F348 F348H F310 FXM-11 FXM-19 F46 Grade 35 Grade 45 Grade 55 Grade 65 Grade 85 — 1B 2A 3A 4A 5A 6A CS Type B DS Type B SS Grade 25 SS Grade 30 SS Grade 33 type 1,2 SS Grade 40 type 1,2 SS Grade 80 HSLAS Grade 70 cl 1 HSLAS Grade 70 cl 2 (Continued)
37
— — S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S32109 S34700 S34709 S34809 S34800 S31000 S21904 S20910 S30600 — — — — — — J93372 J93345 J93371 J92205 J93404 J93380
Plate & Shapes Plate & Shapes Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Line Pipe Line Pipe Line Pipe Line Pipe Line Pipe Structural Shapes Casting Casting Casting Casting Casting Casting Sheet Sheet Sheet Sheet Sheet Sheet Sheet Sheet Sheet
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 2 1 1 1 1 2 1 3 2 3 3 4 4
CS Type A, B, C, D DS Type A, B SS Grade 30 SS Grade 33 SS Grade 36 SS Grade 40 SS Grade 45 SS Grade 50 SS Grade 55 HSLAS Grade 45 cl 1 HSLAS Grade 45 cl 2 HSLAS Grade 50 cl 1 HSLAS Grade 50 cl 2 HSLAS Grade 55 cl 1 HSLAS Grade 55 cl 2 HSLAS Grade 60 cl 1 HSLAS Grade 60 cl 2 HSLAS Grade 65 cl 1 HSLAS Grade 65 cl 2 HSLAS Grade 70 cl 1 HSLAS Grade 70 cl 2
ABS
ABS
1
1
Grade A
K02300
ABS ABS
ABS ABS
1 1
1 1
Grade AH32 Grade B
K11846 K02102
ABS
ABS
1
1
Grade D
K02101
ABS ABS
ABS ABS
1 1
1 1
Grade DH32 Grade E
K11846 K01801
ABS ABS ABS ABS ABS ABS ABS
ABS ABS ABS ABS ABS ABS ABS
1 1 1 1 1 1 1
1 1 2 2 2 2 3
Grade EH32 Grade FH32 Grade AH36 Grade DH36 Grade EH36 Grade FH36 Grade AH40
K11846 K11846 K11852 K11852 K11852 K11852 K11857
ABS
ABS
1
3
Grade DH40
K11857
ABS
ABS
1
3
Grade EH40
K11857
(Continued)
38
Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Ordinary Strength Hull Structural Steel High Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel High Strength Hull Structural Steel Ordinary Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys ABS
ABS
1
3
Grade FH40
K11857
Ordinary Strength Hull Structural Steel
API API API API API API API API API API API API API API API API API
2H 2H 5L 5L 5L 5L 5L 5L 5L 5L 5L 5L 5L 5LS 2Y 2Y 2Y
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 2 1 1 1 1 1 2 2 2 3 3 4 1 1 1 2
Grade 42 Grade 50 Grade A Grade A25, Class I Grade A25, Class II Grade B Grade X42 Grade X52 Grade X56 Grade X60 Grade X65 Grade X70 Grade X80 Grade X46 Grade 42 Grade 50 Grade 50T
— — — — — — — — — — — — — — — — —
Structural Structural Pipe Pipe & Tube Pipe & Tube Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe
AS AS AS AS
1548 1548 1548 1548
1 1 1 1
2 1 2 2
5-490 7-430 7-460 7-490
— — — —
Plate Plate Plate Plate
3678 3678 3678 3678 3678 3678 3678 3679.1 3679.1 3679.1 3679.1 1594 1594 1594 1594 1594 1594
1 1 1 1 1 1 3 1 1 1 1 1 1 1 1 1 1
1 1 1 2 2 2 1 1 2 2 2 1 1 1 1 1 1
200 250 250L15 300/300L15 350/350L15 400/400L15 WR350/WR350L0 250/250L0/250L15 300/300L0/300L15 350/350L0/350L15 400/400L0/400L15 HA1 HA3 HA4N HA200 HA250 HA250/1
— — — — — — — — — — — — — — — — —
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Strip Strip Strip Strip Strip Strip
AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS
(Continued)
39
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA
1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594
1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 3
HU250 HA300 HA300/1 HU300 HU300/1 HA350 HW350 HA400 XF300 XF400 XF500
— — — — — — — — — — —
Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip
G30.18 G30.18 G30.18 G30.18 G30.18 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 Z245.1 Z245.1 Z245.1
1A 1A 1A 1A 1A 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
4 4 4 4 4 1 1 1 1 2 2 2 2 2 2 2 2 2 2 2 3 3 3 3 2 2 2 2 1 1 1
300R 400R 400W 500R 500W 260W 260WT 300W 300WT 350A 350AT 350R 350W 350WT 380W 380WT 400A 400AT 400W 400WT 480W 480WT 480A 480AT 550A 550AT 550W 550WT 172 207 241
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — — —
Rebar Rebar Rebar Rebar Rebar Structural Structural Structural Structural HSLA Steel HSLA Steel HSLA Steel Structural Structural Structural Structural HSLA Steel HSLA Steel HSLA Steel HSLA Steel HSLA Steel HSLA Steel HSLA Steel HSLA Steel Structural Steel Structural Steel Structural Steel Structural Steel Pipe Pipe Pipe
(Continued)
40
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Ferrous Alloys Standard
Base Metal Specification
Material Number
Group Number
Type, Grade, or Alloy Designation
UNS Number
Product Form
Steel and Steel Alloys CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA
Z245.1 Z245.1 Z245.1 Z245.1 Z245.1 Z245.1 Z245.1 Z245.1 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.11 Z245.12 Z245.12 Z245.12 Z245.12 Z245.12 Z245.12 Z245.12 Z245.12
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 2 2 2 3 3 3 4 1 1 1 2 2 2 3 3 3 4 1 1 2 2 2 3 3 3
290 317 359 386 414 448 483 550 207 241 290 317 359 386 414 448 483 550 248 290 317 359 386 414 448 483
— — — — — — — — — — — — — — — — — — — — — — — — — —
Pipe Pipe Pipe Pipe Pipe Pipe Pipe Pipe Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Fittings Steel Flanges Steel Flanges Steel Flanges Steel Flanges Steel Flanges Steel Flanges Steel Flanges Steel Flanges
MSS MSS MSS MSS MSS MSS MSS
SP75 SP75 SP75 SP75 SP75 SP75 SP75
1 1 1 1 1 1 1
1 1 1 2 2 2 3
WPHY-42 WPHY-46 WPHY-52 WPHY-56 WPHY-60 WPHY-65 WPHY-70
— — — — — — —
Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings
41
AWS B2.1/B2.1M-BMG:2009
Table D.1 List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification
Type, Grade, or Alloy Designation
Material UNS Number Number
Product Form
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 351 A 351 A 494 A 494 A 494 A 494 A 494 A 494 A 494 A 494 A 494 A 494
CN7M CT15C Grade N7M Ni-30 Cu (Grade M-35-2) Grade CY-40 Ni-30 Cu-Si-Cb (Grade M-30-C) Ni-30 Cu (Grade M-35-1) Grade CX2MW Grade CW2M Grade CW-6 MC N-7M Grade CW-6M
45 45 44 42 43 42 42 43 43 43 44 43
N08007 N08151 J30007 N04020 N06040 N24130 N24135 N26022 N26455 N26625 N30007 N30107
Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 21 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 42 B 42 B 42 B 42 B 42 B 43 B 68 B 68 B 68 B 68 B 68 B 75 B 75 B 75 B 75 B 75 B 75
Alloy A Naval Brass O60 208.0 (F) 222.0 (T61) 319.0 (F, T5, T6) 328.0 (F, T6) 356.0 (T51, T6, T7, T71) 443.0 (F) 512.0 (F) 514.0 (F) 535.0 (F) 705.0 (T5) 710.0 (T5) A356.0 (T6) B443.0 (F) Deoxidized High P Cu (DHP) Deoxidized Low P Cu (DLP) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (OFXLP) Red Brass, 85% Deoxidized High P Cu (DHP) Deoxidized Low P Cu (DLP) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (OFXLP) Deoxidized High P Cu (DHP) Deoxidized Low P Cu (DLP) Oxygen-Free Cu (DPA) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OFLP)
32 26 26 26 26 26 26 26 26 26 26 26 26 26 31 31 31 31 31 32 31 31 31 31 31 31 31 31 31 31 31
C46400 A02080 A02220 A03190 A03280 A03560 A04430 A05120 A05140 A05350 A07050 A07100 A13560 A24430 C12200 C12000 C10200 C10800 C10300 C23000 C12200 C12000 C10200 C10800 C10300 C12200 C12000 C14200 C10200 C10100 C10800
Rod, Bar & Shapes Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube
(Continued)
42
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 75 B 80 B 80 B 80 B 88 B 88 B 88 B 88 B 90 B 90 B 90 B 90 B 90 B 91 B 91 B 96 B 96 B 96 B 98 B 98 B 98 B 107 B 107 B 107 B 107 B 108 B 108 B 108 B 108 B 108 B 108 B 108 B 108 B 108 B 108 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111
Type, Grade, or Alloy Designation
Material UNS Number Number
Oxygen-Free Cu (OFXLP) AZ91C (-F) AZ92A (-F) KlA (-F) Oxygen Free Cu (DLP) Oxygen Free Cu (DHP) Oxygen Free Cu (OF) Oxygen-Free Cu (OFXLP) AZ31B (-O, H24, H26) AZ31C (-O, H24, H26) HK31A (-O, H24) ZE10A (-O) ZE10A (-O) AZ31B (-F) AZ61A (-F) High Si Bronze A Low Si Bronze B Silicon Bronze High Si Bronze A Low Si Bronze B Silicon Bronze AZ31B (-F) AZ31C (-F) AZ61A (-F) MlA (-F) 308.0 (F) 319.0 (F, T6) 333.0 (T5, T6, T7) 356.0 (F, T51, T6, T7, T71) 443.0 (F) 513.0 (F) 535.0 (F) A356.0 (T61) A444.0 (T4) B443.0 (F) 70-30 Cu-Ni 80-20 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 95-5 Cu-Ni 98.5 min Cu Admiralty, A Admiralty, B Admiralty, C
31 83 83 83 31 31 31 31 81 81 81 81 81 81 81 33 33 33 33 33 33 81 81 81 81 26 26 26 26 26 26 26 26 26 26 34 34 34 34 34 31 32 32 32 (Continued)
43
C10300 M11914 M11920 M18010 C12000 C12200 C10200 C10300 M11311 M11312 M13310 M16100 M16100 M11311 M11610 C65500 C65100 C65400 C65500 C65100 C66100 M11311 M11312 M11610 M15100 A03080 A03190 A03330 A03560 A04430 A05130 A05350 A13560 A14440 A24430 C71500 C71000 C72200 C70600 C70400 C19200 C44300 C44400 C44500
Product Form Seamless Tube Sand Castings Sand Castings Sand Castings Seamless Tube Seamless Tube Seamless Tube Seamless Tube Plate & Sheet Plate & Sheet Plate & Sheet Sheet Plate Forgings Forgings Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Rod, Bars & Shapes Rod, Bars & Shapes Rod, Bars & Shapes Extruded Bars, Rods, Profiles, Tubes, Wires Extruded Bars, Rods, Profiles, Tubes, Wires Extruded Bars, Rods, Profiles, Tubes, Wires Extruded Bars, Rods, Profiles, Tubes, Wires Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 111 B 127 B 135 B 135 B 148 B 148 B 148 B 148 B 148 B 148 B 148 B 148 B 150 B 150 B 150 B 150 B 150 B 150 B 150 B 150 B 150 B 151 B 151 B 152 B 152 B 152 B 152 B 152 B 152 B 152 B 152
Type, Grade, or Alloy Designation
Material UNS Number Number
Aluminum Brass B Aluminum Bronze Aluminum Bronze Aluminum Bronze D Cu-Ni-Fe-Mn Muntz Metal Oxygen-Free Cu (DHP) Oxygen-Free Cu (DLP) Oxygen-Free Cu (DPA) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (OFXLP) Red Brass, 85% Ni-Cu (Alloy 400) Commercial Bronze, 90% Red Brass, 85% Aluminum Bronze Grade A Al-Bronze Grade B Al-Bronze Grade C Al-Bronze Grade D Ni-Al Bronze Grade E, Si-Al Bronze Grade F, Mn-Ni-Al Bronze Ni-Al Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze D 70-30 Cu-Ni 90-10 Cu-Ni Oxygen-Free Cu (DLP) Oxygen-Free Cu (DHP) Oxygen-Free Cu (DPA) Oxygen-Free Cu (DPS) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (OFS)
32 35 35 35 34 32 31 31 31 31 31 31 31 32 42 32 32 35 35 35 35 35 35 35 35 35 35 35 35 35 35 35 35 35 34 34 31 31 31 31 31 31 31 31 (Continued)
44
C68700 C60800 C61300 C61400 C71640 C28000 C12200 C12000 C14200 C10200 C10100 C10800 C10300 C23000 N04400 C22000 C23000 C95410 C95200 C95300 C95400 C95500 C95600 C95700 C95800 C61300 C61900 C62300 C62400 C63000 C63020 C63200 C64200 C61400 C71500 C70600 C12000 C12200 C14200 C12300 C10200 C10100 C10800 C10400
Product Form Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Sheet, Plate, Strip Seamless Tube Seamless Tube Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Rod & Bar Round Rod & Shapes Rod, Bar, Shapes Rod, Bar, Shapes Rod, Bar, Shapes Rod & Bar Rod, Bar, Shapes Rod, Bar, Shapes Round Rod Rod, Bar, Shapes Rod, Bar, Shapes Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 152 B 152 B 152 B 152 B 160 B 160 B 161 B 161 B 162 B 162 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 163 B 164 B 164 B 165 B 166 B 166 B 166 B 166 B 166 B 166 B 167 B 167 B 167 B 167 B 167 B 168 B 168 B 168 B 168 B 168 B 168 B 169 B 169
Type, Grade, or Alloy Designation
Material UNS Number Number
Oxygen-Free Cu (OFS) Oxygen-Free Cu (OFS) Oxygen-Free Cu (OFXLP) Sn Bearing Tellurium Cu 99.0 min Ni (Alloy 200) Lo C-99 min Ni (Alloy 201) 99.0 min Ni (Alloy 200) Lo C-99 min Ni (Alloy 201) 99.0 min Ni (Alloy 200) Lo C-99 min Ni (Alloy 201) 99.0 min Ni (Alloy 200) Lo C-99 min Ni (Alloy 201) Ni-Fe-Cr (Alloy 800) Ni-Fe-Cr (Alloy 801) Ni-Fe-Cr (Alloy 800H) Ni-Fe-Cr (Alloy 800HT) Ni-Cr-Fe (Alloy 6025HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe-Si (Alloy 45) Ni-Cu (30) (Alloy 400) Ni-Fe-Cr (Alloy 825) Ni-Cu (30) (Alloy 400) Ni-Cu (30) (Alloy R 405) Ni-Cu (30) (Alloy 400) Ni-Cr-Co-Mo (Alloy 617) Ni-Cr-Fe (Alloy 6025 HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 601) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe-Si (Alloy 45) Ni-Cr-Fe (Alloy 6025HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 601) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe (Alloy 45) Ni-Cr-Co-Mo (Alloy 617) Ni-Cr-Fe (Alloy 6025 HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 601) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe (Alloy 45) Aluminum Bronze Aluminum Bronze D
31 31 31 31 41 41 41 41 41 41 41 41 45 45 45 45 43 43 43 46 42 45 42 42 42 43 43 43 43 43 46 43 43 43 43 45 43 43 43 43 43 46 35 35 (Continued)
45
C10500 C10700 C10300 C14420 N02200 N02201 N02200 N02201 N02200 N02201 N02200 N02201 N08800 N08801 N08810 N08811 N06025 N06600 N06690 N06045 N04400 N08825 N04400 N04405 N04400 N06617 N06025 N06600 N06601 N06690 N06045 N06025 N06600 N06601 N06690 N06045 N06617 N06025 N06600 N06601 N06690 N06045 C61300 C61400
Product Form Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Plate, Sheet, Strip, Rolled Bar Rod & Bar Rod, Bar, Shapes Seamless Pipe & Tube Seamless Pipe & Tube Sheet, Strip & Plate Sheet, Strip & Plate Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Rod, Bar & Wire Rod, Bar & Wire Seamless Pipe & Tube Rod & Bar Rod & Bar Rod & Bar Rod & Bar Rod & Bar Rod & Bar Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Sheet, Strip & Rolled Bar Sheet, Strip & Rolled Bar
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 170 B 170 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 171 B 187 B 187 B 187 B 187 B 187 B 187 B 187 B 199 B 199 B 199 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209
Type, Grade, or Alloy Designation
Material UNS Number Number
Oxygen-Free Electronic Cu (OF) Oxygen-Free Electronic Cu (OFE) 70-30 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni Admiralty, A Admiralty, B Admiralty, C Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze D Leaded Muntz Metal Naval Brass Naval Brass, Arsenical Controlled Oxygen Cu Oxygen-Free Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu with Ag (OFS) Oxygen-Free Cu with Ag (OFS) Sn Bearing Tellurium Cu AM100A (-F) AZ91C (-F) AZ92A (-F) 1060 1100 2014 (T3, T4, T45, T6, T65) 2219 (T31, T37, T62, T81, T87) 3003 3004 3005 3105 5005 5010 5050 5052 5083 5086 5154 5252 5254 5454 5456
31 31 34 34 34 32 32 32 35 35 35 35 32 32 32 31 31 31 31 31 31 31 83 83 83 21 21 24 24 21 22 21 21 21 21 21 22 25 25 22 22 22 22 25
(Continued)
46
C10200 C10100 C71500 C72200 C70600 C44300 C44400 C44500 C61300 C63000 C63200 C61400 C36500 C46400 C46500 C10940 C10200 C10100 C10300 C10400 C10700 C14420 M10100 M11914 M11920 A91060 A91100 A92014 A92219 A93003 A93004 A93005 A93105 A95005 A95010 A95050 A95052 A95083 A95086 A95154 A95252 A95254 A95454 A95456
Product Form Refinery Shapes Refinery Shapes Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Rod, Bar & Rolled Shapes Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Sheet Sheet Plate & Sheet Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 209 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 211 B 211 B 211 B 211 B 211 B 211 B 211 B 211 B 211 B 211 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221
Type, Grade, or Alloy Designation
Material UNS Number Number
5457 5652 6061 (T4, T6, T651) Alclad 2014 (T3, T4, T45, T6, T65) Alclad 2219 (T31, T37, T62, T81, T87) Alclad 3003 Alclad 3004 Alclad 6061 (T4, T6, T62, T651) 3303 1060 1100 2014 (T4, T6) 3003 3102 5005 5050 5052 5083 5086 5154 5456 6061 (T4, T6) 6063 (T4, T6, T62, T83) Alclad 3003 Alclad 3102 Alclad 3303 1060 1100 2014 (T4, T6) 2219 (T851) 3003 5052 5056 5154 6061 (T4, T6, T62, T651) Alclad 5056 1060 1100 2014 (T4, T45, T6, T65) 2219 (T31, T35, T62, T81, T85) 3003 3004 3102 5052
21 22 23 24 24 21 22 23 21 21 21 24 21 21 21 21 22 25 25 22 25 23 23 21 21 21 21 21 24 24 21 22 25 22 23 25 21 21 24 24 21 22 21 22
(Continued)
47
A95457 A95652 A96061 A82014 A82219 A83003 A83004 A86061 A93303 A91060 A91100 A92014 A93003 A93102 A95005 A95050 A95052 A95083 A95086 A95154 A95456 A96061 A96063 A83003 A83102 A83303 A91060 A91100 A92014 A92219 A93003 A95052 A95056 A95154 A96061 A85056 A91060 A91100 A92014 A92219 A93003 A93004 A93102 A95052
Product Form Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire Bar, Rod & Wire Bar, Rod & Wire Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire Bar, Rod & Wire (Cold Finished) Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 221 B 230 B 234 B 234 B 234 B 234 B 234 B 234 B 236 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 241 B 247 B 247 B 247 B 247 B 247 B 247
Type, Grade, or Alloy Designation
Material UNS Number Number
5083 5086 5154 5454 5456 6005 (T1, T5) 6005A (T1, T5) 6061 (T1, T4, T5, T6, T651) 6063 (T1, T4, T5, T6) 6105 (T1, T5) 6162 (T5, T55, T6, T65) 6351 (T1, T4, T5, T6) 6463 (T1, T5, T6) 7005 (T53) Alclad 3003 1350 1060 3003 5052 5454 6061 (T4, T6) Alclad 3003 1350 6063 (T1, T4, T42,T5, T52, T6, T62) 1060 1100 2014 (T4, T45, T6, T62, T65) 2219 (T31, T35, T62, T81, T85) 3003 5052 5083 5086 5454 5456 6061 (T1, T4, T42, T51, T6, T62) 6162 (T5, T55, T6, T65) 6351 (T4, T6) Alclad 3003 1100 2014 (T4, T6) 2014 (T6, T652) 2219 (T6) 2219 (T6, T852) 3003
25 25 22 22 25 23 23 23 23 23 23 23 23 27* 21 21 21 21 22 22 23 21 21 23 21 21 24 24 21 22 25 25 22 25 23 23 23 21 21 24 24 24 24 21
(Continued)
48
A95083 A95086 A95154 A95454 A95456 A96005 A96005 A96061 A96063 A96105 A96162 A96351 A96463 A97005 A83003 A91350 A91060 A93003 A95052 A95454 A96061 A83003 A91350 A96063 A91060 A91100 A92014 A92219 A93003 A95052 A95083 A95086 A95454 A95456 A96061 A96162 A96351 A83003 A91100 A92014 A92014 A92219 A92219 A93003
Product Form Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Wire (Electrical) Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tubes Drawn Seamless Tubes Drawn Seamless Tube Drawn Seamless Tube Bars (Electrical) Extruded Seamless Pipe & Tube Seamless Pipe & Ext. Tube Seamless Pipe & Ext. Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Seamless Pipe & Ext. Tube Extruded Seamless Pipe & Tube Ext. Pipe & Tube Ext. Pipe & Tube Extruded Seamless Pipe & Tube Ext. Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Seamless Pipe & Ext. Tube Die, Hand & Rolled Ring Forgings Die Forgings H& Forgings Die Forgings H& Forgings Die, Hand & Rolled Ring Forgings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 247 B 247 B 247 B 247 B 247 B 247 B 247 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 271 B 271 B 271 B 271 B 271 B 280
Type, Grade, or Alloy Designation
Material UNS Number Number
5083 5083 6061 (T6) 6061 (T6, T652) 6061 (T6, T652) 6151 (T6) 6151 (T6, T652) Grade 1 Grade 2 Grade 3 Grade 4 Grade 5 Grade 6 Grade 7 Grade 9 Grade 11 Grade 12 Grade 13 Grade 14 Grade 15 Grade 16 Grade 17 Grade 18 Grade 19 Grade 20 Grade 21 Grade 24 Grade 25 Grade 26 Grade 27 Grade 28 Grade 29 Grade 30 Grade 31 Grade 32 Grade 33 Grade 34 Grade 35 Aluminum Bronze Grade A Al-Bronze Grade B Al-Bronze Grade C Al-Bronze Grade D Ni-Al Bronze Deoxidized Cu (DHP)
25 25 23 23 23 23 23 51 51 52 53 54 54 51 53 51 52 51 52 52 51 51 53 53 53 53 54 54 51 51 53 54 51 52 53 51 52 54 35 35 35 35 35 31 (Continued)
49
A95083 A95083 A96061 A96061 A96061 A96151 A96151 R50250 R50400 R50550 R50700 R56400 R54520 R52400 R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 R58640 R58645 R58210 R56405 R56403 — — R56323 R56404 — — — — — — C95410 C95200 C95300 C95400 C95500 C12200
Product Form H& Forgings Die Forgings Die Forgings Rolled Ring Forgings H& Forgings Die Forgings Rolled Ring Forgings Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Centrifugal Castings Centrifugal Castings Centrifugal Castings Centrifugal Castings Centrifugal Castings Seamless Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 280 B 280 B 283 B 283 B 308 B 313 B 313 B 313 B 313 B 313 B 313 B 313 B 313 B 313 B 313 B 315 B 315 B 315 B 315 B 315 B 315 B 317 B 324 B 333 B 333 B 333 B 333 B 333 B 335 B 335 B 335 B 335 B 335 B 337 B 337 B 337 B 337 B 337 B 337 B 337 B 338 B 338 B 338 B 338
Type, Grade, or Alloy Designation
Material UNS Number Number
Deoxidized Cu (DLP) Oxygen-free Cu (OF) Al-Si Bronze High Si Bronze A 6061 (T6) 1100 3003 3004 3005 5050 5052 5086 5154 6061 (T4, T6) Alclad 3004 Aluminum Bronze Aluminum Bronze D High Si Bronze A High Si Bronze A Low Si Bronze B Low Si Bronze B 6101 (T6, T61, T64, T65) 1350 Ni-Mo-Fe (Alloy B) Alloy B-10 Ni-Mo-Fe (Alloy B-4) Ni-Mo (Alloy B-2) Ni-Mo-Cr-Fe (Alloy B-3) Ni-Mo-Fe (Alloy B) Alloy B-10 Ni-Mo-Fe (Alloy B-4) Ni-Mo (Alloy B-2) Ni-Mo-Cr-Fe (Alloy B-3) Grade 1 Grade 2 Grade 3 Grade 7 Grade 9 Grade 11 Grade 12 Grade 1 Grade 2 Grade 3 Grade 7
31 31 35 33 23 21 21 22 21 21 22 25 22 23 22 35 35 33 33 33 33 23 21 44 44 44 44 44 44 44 44 44 44 51 51 52 51 53 51 52 51 51 52 51 (Continued)
50
C12000 C10200 C64200 C65500 A96061 A91100 A93003 A93004 A93005 A95050 A95052 A95086 A95154 A96061 A83004 C61300 C61400 C65500 C65500 C65100 C65100 A96101 A91350 N10001 N10624 N10629 N10665 N10675 N10001 N10624 N10629 N10665 N10675 R50250 R50400 R50550 R52400 R56320 R52250 R53400 R50250 R50400 R50550 R52400
Product Form Seamless Tube Seamless Tube Die Forgings Die Forgings Standard Structural Shapes Welded Tube Welded Tube Formed Sheet & Seam Welded Tube Welded Tube Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Seamless Pipe Seamless Pipe Pipe Tube Pipe Tube Ext. Bar, Rod, Wire, Shapes & Tube Rectangular & Square Wire (Electrical) Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Rod Rod Rod Rod Rod Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 345 B 345 B 345 B 345 B 345 B 345 B 345 B 345 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348
Type, Grade, or Alloy Designation
Material UNS Number Number
Grade 9 Grade 11 Grade 12 Grade 13 Grade 14 Grade 15 Grade 16 Grade 17 Grade 18 Grade 27 Grade 28 Grade 30 Grade 31 Grade 33 Grade 34 Grade 35 1060 3003 5083 5086 6061 (T4, T45, T6, T65) 6063 (T1, T4, T5, T6) 6351 (T4, T6) Alclad 3003 Grade 1 Grade 2 Grade 3 Grade 4 (Unalloyed Ti) Grade 5 Grade 6 Grade 7 Grade 9 Grade 11 Grade 12 Grade 13 Grade 14 Grade 15 Grade 16 Grade 17 Grade 18 Grade 19 Grade 20 Grade 21 Grade 23
53 51 52 51 52 52 51 51 53 51 53 51 52 51 52 54 21 21 25 25 23 23 23 21 51 51 52 53 54 54 51 53 51 52 51 52 52 51 51 53 53 53 53 54 (Continued)
51
R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 — R56323 — — — — — A91060 A93003 A95083 A95086 A96061 A96063 A96351 A83003 R50250 R50400 R50550 R50700 R56400 R54520 R52400 R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 R58640 R58645 R58210 R56402
Product Form Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless Pipe & Tube (Gas & Oil Trans.) Seamless Pipe & Tube (Gas & Oil Trans.) Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Seamless Pipe & Tube (Gas & Oil Trans.) Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 351 B 351 B 351 B 351 B 352 B 352 B 352 B 352 B 353 B 353 B 353 B 353 B 353 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 359 B 361 B 361 B 361 B 361
Type, Grade, or Alloy Designation
Material UNS Number Number
Grade 24 Grade 25 Grade 30 Grade 31 Grade 32 Grade 33 Grade 34 Grade 35 R60001 R60802 R60804 R60901 R60001 R60802 R60804 R60901 R60001 R60802 R60804 R60901 R60904 70-30 Cu-Ni 80-20 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 95-5 Cu-Ni 98.7 min Cu Admiralty, A Admiralty, B Admiralty, C Aluminum Brass B Aluminum Bronze Deoxidized As-Cu (DPA) Deoxidized High P Cu (DHP) Deoxidized Low P Cu (DLP) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OFXLP) Oxygen-Free Low P Cu (OFLP) Red Brass, 85% Alclad 3003 WP1060 WP1100 WP3003
54 54 51 52 53 52 52 54 61 61 61 62 61 61 61 62 61 61 61 62 62 34 34 34 34 34 31 32 32 32 32 35 31 31 31 31 31 31 31 32 21 21 21 21
(Continued)
52
R56405 R56403 — — — — — — R60001 R60802 R60804 R60901 R60001 R60802 R60804 R60901 R60001 R60802 R60804 R60901 R60904 C71500 C71000 C72200 C70600 C70400 C19200 C44300 C44400 C44500 C68700 C60800 C14200 C12200 C12000 C10200 C10100 C10300 C10800 C23000 A83003 A91060 A91100 A93003
Product Form Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars, Rod, Wire Bars, Rod, Wire Bars, Rod, Wire Bars, Rod, Wire Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Fittings Fittings Fittings Fittings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 361 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 363 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366
Type, Grade, or Alloy Designation
Material UNS Number Number
WP5154 WPT 1 WPT 2 WPT 3 WPT 7 WPT 9 WPT 11 WPT 12 WPT 13 WPT 14 WPT 15 WPT 16 WPT 17 WPT 18 WPT 19 WPT 20 WPT 21 WPT 23 WPT 24 WPT 25 WPT 30 CR1925 CR1925N CR20CB CR3033 CR3127 CR330 CR5923 CR603GT CR6XN CR904L CRB10 CRH120 CRH160 CRH230 CRH556 CRHB CRHB2 CRHB3 CRHC2000 CRHC22 CRHC276 CRHC4 CRHG
22 51 51 52 51 53 51 52 51 52 52 51 51 53 53 53 53 54 54 54 51 45 45 44 45 45 46 44 43 45 45 44 45 44 47 45 44 44 44 44 44 44 44 45 (Continued)
53
A95154 R50250 R50400 R50550 R52400 R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 R58640 R58645 R58210 R56402 R56405 R56403 — N08925 N08926 N08020 R20033 N08031 N08330 N06059 N06603 N08367 N08904 N10624 N08120 N12160 N06230 R30556 N10001 N10665 N10675 N06200 N06022 N10276 N06455 N06007
Product Form Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366
Type, Grade, or Alloy Designation
Material UNS Number Number
CRHG3 CRHG30 CRHN CRHX CRM21 CRN CRN1C10 CRN1C11 CRN1CMC CRNC CRNCI CRNCMC CRNIC CRNL CRV45TM CRV602 CRVB4 WP1925 WP1925N WP20CB WP3127 WP330 WP5923 WP603GT WP6XN WP904L WPB10 WPH120 WPH160 WPH230 WPH556 WPHB WPHB-2 WPHB-3 WPHC2000 WPHC22 WPHC276 WPHC4 WPHG WPHG3 WPHG30 WPHN WPHX WPM21
45 45 44 43 44 41 45 45 45 42 43 43 44 41 46 43 44 45 45 44 45 46 44 43 45 45 44 45 44 47 45 44 44 44 44 44 44 44 45 45 45 44 43 44 (Continued)
54
N06985 N06030 N10003 N06002 N06210 N02200 N08810 N08811 N08825 N04400 N06600 N06625 N08800 N02201 N06045 N06025 N10629 N08925 N08926 N08020 N08031 N08330 N06059 N06603 N08367 N08904 N10624 N08120 N12160 N06230 R30556 N10001 N10665 N10675 N06200 N06022 N10276 N06455 N06007 N06985 N06030 N10003 N06002 N06210
Product Form Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification
Type, Grade, or Alloy Designation
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
WPN WPN1C10 WPN1C11 WPN1CMC WPNC WPNCI WPNCMC WPNIC WPNL WPV45TM WPV602 WPVB24 Pd 16 Pd 17 Pd 7B Pd 8A Grade C-2 Grade C-3 Grade C-5 Grade C-6 F-1 F-2 F-3 F-4 (Unalloyed Ti) F-5 F-6 F-7 F-9 F-11 F-12 F-13 F-14 F-15 F-16 F-17 F-18 F-19 F-20 F-21 F-23 F-24 F-25 F-30 F-31
B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 367 B 367 B 367 B 367 B 367 B 367 B 367 B 367 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381
Material UNS Number Number 41 45 45 45 42 43 43 44 41 46 43 44 51 51 51 52 51 52 54 54 51 51 52 53 54 54 51 53 51 52 51 52 52 51 51 53 53 53 53 54 54 54 51 52 (Continued)
55
N02200 N08810 N08811 N08825 N04400 N06600 N06625 N08800 N02201 N06045 N06025 N10629 R52402 R52252 R52401 R52401 R50400 R50550 R56400 R54520 R50250 R50400 R50550 R50700 R56400 R54520 R52400 R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 R58640 R58645 R58210 R56402 R56405 R56403 — —
Product Form Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings (Solution Treated) Forgings (Solution Treated) Forgings (Solution Treated) Forgings Forgings Forgings Forgings Forgings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 395 B 396 B 403 B 403 B 403 B 403 B 407 B 407 B 407 B 407 B 407 B 408 B 408 B 408 B 408 B 409 B 409 B 409 B 409 B 423 B 423 B 424 B 424 B 425 B 425 B 429 B 429
Type, Grade, or Alloy Designation
Material UNS Number Number
70-30 Cu-Ni 80-20 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 95-5 Cu-Ni 98.7 min Cu Admiralty, A Admiralty, B Admiralty, C Aluminum Brass B Aluminum Bronze Deoxidized As-Cu (DPA) Deoxidized High P Cu (DHP) Deoxidized Low P Cu (DLP) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Low P Cu (OFLP) Red Brass, 85% 5005 AM100A (-F) AZ91C(-F) AZ92A(-F) K1A(-F) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 801) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800HT) Ni-Fe-Cr (Alloy HR120) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800HT) Ni-Fe-Cr (Alloy HR120) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800HT) Ni-Fe-Cr (Alloy HR120) Ni-Fe-Cr-Mo-Cu (Alloy 20Cb3Mod.) Ni-Fe-Cr-Mo-Cu (Alloy 825) Ni-Fe-Cr-Mo-Cu (Alloy 20Cb3Mod.) Ni-Fe-Cr-Mo-Cu (Alloy 825) Ni-Fe-Cr-Mo-Cu (Alloy 20Cb3Mod.) Ni-Fe-Cr-Mo-Cu (Alloy 825) 6061 (T6) 6063 (T6)
34 34 34 34 34 31 32 32 32 32 35 31 31 31 31 31 31 32 21 83 83 83 83 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 23 23
(Continued)
56
C71500 C71000 C72200 C70600 C70400 C19200 C44300 C44400 C44500 C68700 C60800 C14200 C12200 C12000 C10200 C10300 C10800 C23000 A95005 M10100 M11914 M11920 M18010 N08800 N08801 N08810 N08811 N08120 N08800 N08810 N08811 N08120 N08800 N08810 N08811 N08120 N08221 N08825 N08221 N08825 N08221 N08825 A96061 A96063
Product Form Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Wire (Electrical) Investment Castings Investment Castings Investment Castings Investment Castings Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Rod & Bar Rod & Bar Rod & Bar Rod & Bar Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Rod & Bar Rod & Bar Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 434 B 435 B 435 B 435 B 435 B 443 B 443 B 444 B 444 B 446 B 446 B 462 B 462 B 462 B 462 B 462 B 463 B 463 B 463 B 464 B 464 B 464 B 466 B 466 B 466 B 466 B 466 B 467 B 467 B 468 B 468 B 468 B 473 B 473 B 473 B 483 B 483 B 483 B 483 B 483 B 483 B 483 B 483 B 483
Type, Grade, or Alloy Designation
Material UNS Number Number
Ni-Mo-Cr (Alloy N) Fe-Cr-Ni-Co-Mo-W (Alloy 556) Ni-Co-Cr-Si (Alloy HR160) Ni-Cr-Fe-Mo (Alloy X) Ni-Cr-W-Mo (Alloy 230) Alloy 625, Grade 1 Alloy 625, Grade 2 Ni-Cr-Mo-Cb (Alloy 625) Grade 1 Ni-Cr-Mo-Cb (Alloy 625) Grade 2 Ni-Cr-Mo-Cb (Alloy 625) Grade 1 Ni-Cr-Mo-Cb (Alloy 625) Grade 2 Cr-Ni-Fe (Alloy 33) Fe-Ni-Cr-Mo (Alloy 6XN) Ni-Fe-Cr-Cu-Mo (Alloy 20Cb3) Ni-Fe-Cr-Mo-Cu (Alloy 20Mo-4) Ni-Fe-Cr-Mo-Cu (Alloy 20 Mo-6) Ni-Fe-Cr-Cu-Mo (Alloy 20Cb3) Ni-Fe-Cr-Mo-Cu (Alloy 20Mo-4) Ni-Fe-Cr-Mo-Cu (Alloy 20 Mo-6) Ni-Fe-Cr-Cu-Mo (Alloy 20Cb3) Ni-Fe-Cr-Mo-Cu (Alloy 20Mo-4) Ni-Fe-Cr-Mo-Cu (Alloy 20 Mo-6) 70-30 Cu-Ni 80-20 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 95-5 Cu-Ni 70-30 Cu-Ni 90-10 Cu-Ni Ni-Fe-Cr-Cu-Mo (Alloy 20Cb3) Ni-Fe-Cr-Mo-Cu (Alloy 20Mo-4) Ni-Fe-Cr-Mo-Cu (Alloy 20 Mo-6) Ni-Fe-Cr-Cu-Mo (Alloy 20Cb3) Ni-Fe-Cr-Mo-Cu (Alloy 20Mo-4) Ni-Fe-Cr-Mo-Cu (Alloy 20 Mo-6) 1060 1100 1435 3003 3102 5005 5050 5052 6061 (T4, T6)
44 45 46 43 43 43 43 43 43 43 43 45 45 45 45 45 45 45 45 45 45 45 34 34 34 34 34 34 34 45 45 45 45 45 45 21 21 21 21 21 21 21 22 23
(Continued)
57
N10003 R30556 N12160 N06002 N06230 N06625 N06625 N06625 N06625 N06625 N06625 R20033 N08367 N08020 N08024 N08026 N08020 N08024 N08026 N08020 N08024 N08026 C71500 C71000 C72200 C70600 C70400 C71500 C70600 N08020 N08024 N08026 N08020 N08024 N08026 A91060 A91100 A91435 A93003 A93102 A95005 A95050 A95052 A96061
Product Form Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Cold Rolled Strip & Sheet Plate & Hot Rolled Sheet (Sol. Anneal) Pipe & Tube Pipe & Tube Rod & Bar Rod & Bar Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Pipe Welded Pipe Welded Pipe Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Bars Bars Bars Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose)
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 483 B 491 B 491 B 491 B 491 B 491 B 491 B 491 B 493 B 493 B 493 B 505 B 511 B 511 B 512 B 514 B 514 B 514 B 515 B 515 B 515 B 515 B 516 B 516 B 516 B 516 B 517 B 517 B 517 B 517 B 523 B 523 B 523 B 535 B 535 B 536 B 536 B 543 B 543 B 543 B 543 B 543 B 543 B 543
Type, Grade, or Alloy Designation
Material UNS Number Number
6063 (T4, T6) 1050 1100 1200 1235 3003 3102 6063 (T1) R60702 R60704 R60705 Grade A Al-Bronze Ni-Fe-Cr-Si (Alloy 330) Ni-Fe-Cr-Si (Alloy 330 TX) Alloy 330 Ni-Fe-Cr (Alloy HR120) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800HT) Ni-Fe-Cr (Alloy HR120) Ni-Cr-Fe (Alloy 6025 HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe-Si (Alloy 45) Alloy 603 GT Ni-Cr-Fe (Alloy 6025 HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe-Si (Alloy 45) Alloy 603GT R60702 R60704 R60705 Ni-Fe-Cr-Si (Alloy 330) Ni-Fe-Cr-Si (Alloy 330TX) Ni-Fe-Cr-Si (Alloy 330) Ni-Fe-Cr-Si (Alloy 330TX) 70-30 Cu-Ni 80-20 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 95-5 Cu-Ni 97.0 min Cu Admiralty, A
23 21 21 21 21 21 21 23 61 61 62 35 45 45 45 45 45 45 45 45 45 45 43 43 46 43 43 43 46 43 61 61 62 45 45 45 45 34 34 34 34 34 31 32 (Continued)
58
A96063 A91050 A91100 A91200 A91235 A93003 A93102 A96063 R60702 R60704 R60705 C95200 N08330 N08332 N08330 N08120 N08800 N08810 N08800 N08810 N08811 N08120 N06025 N06600 N06045 N06603 N06025 N06600 N06045 N06603 R60702 R60704 R60705 N08330 N08332 N08330 N08332 C71500 C71000 C72200 C70600 C70400 C19400 C44300
Product Form Drawn Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Forgings Forgings Forgings Continuous Casting Repair Bars & Shapes Bars & Shapes Billets & Bars Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Pipe Welded Pipe Welded Pipe Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 543 B 543 B 543 B 543 B 543 B 543 B 543 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 547 B 550 B 550 B 550 B 551 B 551 B 551 B 551 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564
Type, Grade, or Alloy Designation
Material UNS Number Number
Admiralty, B Admiralty, C Aluminum Brass B Cu-Ni-Fe-Mn Deoxidized High P Cu (DHP) Oxygen-Free Low P Cu (OFLP) Red Brass, 85% 1100 3003 3004 5050 5052 5083 5086 5154 5454 6061 (T4, T6) Alclad 3003 Alclad 3004 R60702 R60704 R60705 R60702 R60704 R60705 R60706 99.0 min Ni (Alloy 200) Ni-30 Cu (Alloy 400) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C-22) Ni-Cr-Fe-Al (Alloy 6025 HT) Ni-Cr-Fe-Si (Alloy 45) Ni-Cr-Mo-(Lo C) (Alloy 59) Ni-Cr-Mo-W Alloy C2000 Alloy 21 Ni-Cr-W-Mo (Alloy 230) Ni-Cr-Fe (Alloy 600) Alloy 603GT Ni-Cr-Co-Mo (Alloy 617) Ni-Cr-Mo-Cb (Alloy 625) Ni-Cr-Mo-W-(Lo C) (Alloy 686) Ni-Cr-Fe (Alloy 690) Fe-Ni-Cr-Mo-Cu (Alloy 31) Ni-Fe-Cr (Alloy HR120)
32 32 32 34 31 31 32 21 21 22 21 22 25 25 22 22 23 21 22 61 61 62 61 61 62 62 41 42 43 43 46 43 43 43 43 43 43 43 43 43 44 43 45 45
(Continued)
59
C44400 C44500 C68700 C71640 C12200 C10800 C23000 A91100 A93003 A93004 A95050 A95052 A95083 A95086 A95154 A95454 A96061 A83003 A83004 R60702 R60704 R60705 R60702 R60704 R60705 R60706 N02200 N04400 N06022 N06025 N06045 N06059 N06110 N06200 N06210 N06230 N06600 N06603 N06617 N06625 N06686 N06690 N08031 N08120
Product Form Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Roll Formed & Long. Welded Tube Roll Formed & Long. Welded Tube Formed Sheet & Arc Welded Tube Roll Formed & Long. Welded Tube Formed Sheet & Arc Welded Tube Formed & Arc Seam Welded Tube Formed & Arc Seam Welded Tube Formed Sheet & Arc Welded Tube Formed Sheet & Arc Welded Tube Formed & Arc Seam Welded Tube Roll Formed & Long. Welded Tube Formed Sheet & Arc Welded Tube Bars, Shapes & Wire Bars, Shapes & Wire Bars, Shapes & Wire Sheet, Strip, Plate Sheet, Strip, Plate Sheet, Strip, Plate Sheet, Strip, Plate Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 572 B 572 B 572 B 572 B 573 B 574 B 574 B 574 B 574 B 574 B 574 B 575 B 575 B 575 B 575 B 575 B 575 B 581 B 581 B 581 B 581 B 582 B 582 B 582 B 582 B 599 B 608 B 608 B 608 B 608 B 609 B 618
Type, Grade, or Alloy Designation
Material UNS Number Number
Fe-Ni-Cr-Mo (Alloy AL-6XN) Fe-Ni-Cr (Alloy 800) Fe-Ni-Cr (Alloy 800H) Fe-Ni-Cr (Alloy 800HT) Ni-Fe-Cr-Mo-C (Alloy 825) Ni-Mo-Cr-Fe-W (Alloy C-276) Alloy B-10 Alloy CRB10 Ni-Mo-Fe (Alloy B-4) Ni-Mo-Cr-Fe (Alloy B-3) Ni-Co-Cr-Si (Alloy HR160) Cr-Ni-Fe (Alloy 33) Ni-Cr-Fe-Mo (Alloy X) Ni-Cr-W-Mo (Alloy 230) Ni-Co-Cr-Si (Alloy HR160) Fe-Cr-Ni-Co-Mo-W (Alloy 556) Ni-Mo-Cr-Fe (Alloy N) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C22) Ni-Cr-Mo-(Lo C) (Alloy 59) Alloy C2000 Ni-Cr-Mo-(Lo C) (Alloy C-4) Ni-Cr-Mo-W-(Lo C) (Alloy C686) Ni-Mo-Cr-Fe-W-(Lo C) (Alloy C-276) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C22) Ni-Cr-Mo-(Lo C) (Alloy 59) Alloy C2000 Ni-Cr-Mo-(Lo C) (Alloy C-4) Ni-Cr-Mo-W-(Lo C) (Alloy 686) Ni-Mo-Cr-Fe-W-(Lo C) (Alloy C-276) Ni-Cr-Fe-Mo-Cu (Alloy G) Ni-Cr-Fe-Mo-W-Cu (Alloy G-30) Ni-Cr-Fe-Mo-Ti (Alloy G-2) Ni-Cr-Fe-Mo-Cu (Alloy G-3) Ni-Cr-Fe-Mo-Cu (Alloy G) Ni-Cr-Fe-Mo-W-Cu (Alloy G-30) Ni-Cr-Fe-Mo-Ti (Alloy G-2) Ni-Cr-Fe-Mo-Cu (Alloy G-3) Alloy 700 70-30 Cu-Ni 90-10 Cu-Ni Aluminum Bronze Aluminum Bronze D 1350 208.0 (F)
45 45 45 45 45 43 43 43 44 44 46 45 43 43 46 45 44 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 45 34 34 35 35 21 26
(Continued)
60
N08367 N08800 N08810 N08811 N08825 N10276 N10624 N10624 N10629 N10675 N12160 R20033 N06002 N06230 N12160 R30556 N10003 N06022 N06059 N06200 N06455 N06686 N10276 N06022 N06059 N06200 N06455 N06686 N10276 N06007 N06030 N06975 N06985 N06007 N06030 N06975 N06985 N08700 C71520 C70620 C61300 C61400 A91350 A02080
Product Form Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Rod Rod Rod Rod Rod Rod Rod Rod Rod Rod Rod Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Rod Rod Rod Rod Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Pipe Welded Pipe Welded Pipe Welded Pipe Wire (Electrical) Investment Castings
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 618 B 618 B 618 B 618 B 618 B 618 B 618 B 618 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 620 B 621 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622
Type, Grade, or Alloy Designation
Material UNS Number Number
319.0 (F, T6) 328.0 (F, T6) 356.0 (T6, T7, T51, T71) 443.0 (F) 514.0 (F) 535.0 (F) A356.0 (T6) B443.0 (F) Ni-Cr-Fe-Mo (Alloy X) Ni-Cr-Fe-Mo-Cu (Alloy G) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C-22) Ni-Cr-Fe-Mo-Cu (Alloy G-30) Ni-Cr-Mo (Alloy 59) Alloy C2000 Ni-Cr-W-Mo (Alloy 230) Ni-Cr-Mo (Alloy C-4) Ni-Cr-Mo-W (Alloy 686) Ni-Cr-Fe-Mo (Alloy G-2) Ni-Cr-Fe-Mo-Cu (Alloy G-3) Fe-Ni-Cr-Mo-Cu (Alloy 31) Fe-Ni-Cr-Mo (Alloy 20 Mod.) Ni-Mo-Fe (Alloy B) Ni-Mo-Cr-Fe-W (Alloy C-276) Alloy B-10 Ni-Mo-Fe-Cr (Alloy B-4) Ni-Mo (Alloy B-2) Ni-Mo-Cr-Fe (Alloy B-3) Ni-Co-Cr-Si (Alloy HR160) Cr-Ni-Fe (Alloy 33) Fe-Cr-Ni-Co-Mo-W (Alloy 556) Fe-Ni-Cr-Mo (Alloy 20 Mod.) Fe-Ni-Cr-Mo (Alloy 20 Mod.) Ni-Cr-Fe-Mo (Alloy X) Ni-Cr-Fe-Mo-Cu (Alloy G) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C-22) Ni-Cr-Fe-Mo-W-Cu (Alloy G-30) Ni-Cr-Mo-Fe (Alloy 59) Ni-Cr-Mo-Fe (Alloy 2060 Mo) Alloy C2000 Ni-Cr-W-Mo (Alloy 230) Ni-Cr-Mo (Alloy 2050) Ni-Cr-Fe-Mo-W (Alloy 2550) Ni-Cr-Mo-W (Alloy 686) Ni-Cr-Fe-Mo-Ti (Alloy G-2)
26 26 26 26 26 26 26 26 43 43 43 43 43 43 43 43 43 43 43 45 45 44 43 44 44 44 44 46 45 45 45 45 43 43 43 43 43 43 43 43 43 43 43 43
(Continued)
61
A03190 A03280 A03560 A04430 A05140 A05350 A13560 A24430 N06002 N06007 N06022 N06030 N06059 N06200 N06230 N06455 N06686 N06975 N06985 N08031 N08320 N10001 N10276 N10624 N10629 N10665 N10675 N12160 R20033 R30556 N08320 N08320 N06002 N06007 N06022 N06030 N06059 N06060 N06200 N06230 N06250 N06255 N06686 N06975
Product Form Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Plate, Sheet & Strip Rod Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 625 B 625 B 625 B 625 B 625 B 625 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 632 B 649
Type, Grade, or Alloy Designation
Material UNS Number Number
Ni-Cr-Fe-Mo-Cu (Alloy G-3) Fe-Ni-Cr-Mo-Cu (Alloy 31) Fe-Ni-Cr-Mo-W (Alloy 2035) Fe-Ni-Cr-Mo (Alloy 20 Mod.) Fe-Ni-Cr-Mo-Cu Ni-Mo-Fe (Alloy B) Ni-Mo-Cr-Fe-W (Alloy C-276) Alloy B-10 Ni-Mo-Fe-Cr (Alloy B-4) Ni-Mo (Alloy B-2) Ni-Mo-Cr-Fe (Alloy B-3) Ni-Co-Cr-Si (Alloy HR160) Cr-Ni-Fe-Mo (Alloy 33) Fe-Cr-Ni-Co-Mo-W (Alloy 556) Fe-Ni-Cr-Mo-Cu (Alloy 31) Fe-Ni-Cr-Mo (Alloy 904L) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 1925) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 926) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy UR-SB-8) Cr-Ni-Fe-Mo (Alloy 33) Ni-Cr-Fe-Mo Ni-Cr-Fe-Mo (Alloy G) Ni-Cr-Mo-(Lo C)-4Fe-3W (Alloy C-22) Ni-Cr-Fe-Mo (Alloy G30) Ni-Cr-Mo (Alloy 59) Ni-Cr-Mo-(Low C)-Cu (Alloy C2000) Ni-Cr-W-Mo (Alloy 230) Ni-Cr-Mo (Alloy C-4) Ni-Cr-Mo-W (Alloy 686) Ni-Cr-Fe-Mo-Ti (Alloy G-2) Ni-Cr-Fe-Mo-Cu (Alloy G-3) Fe-Ni-Cr-Mo-Cu (Alloy 31) Fe-Ni-Cr-Mo (Alloy 20 Mod.) Ni-Mo-Fe (Alloy B) Ni-Mo-Cr-Fe-W (Alloy C-276) Alloy B-10 Ni-Mo-Fe (Alloy B-4) Ni-Mo (Alloy B-2) Ni-Mo-Cr-Fe (Alloy B-3) Ni-Co-Cr-Si (Alloy HR160) Fe-Cr-Ni-Mo (Alloy 33) Fe-Cr-Ni-Co-Mo-W (Alloy 556) 6061 (T4, T6) Ni-Fe-Cr-Mo-Cu (Alloy 31)
43 45 45 45 45 44 43 44 44 44 44 46 45 45 45 45 45 45 45 45 43 43 43 43 43 43 43 43 43 43 43 45 45 44 43 44 44 44 44 46 45 45 23 45
(Continued)
62
N06985 N08031 N08135 N08320 N08535 N10001 N10276 N10624 N10629 N10665 N10675 N12160 R20033 R30556 N08031 N08904 N08925 N08926 N08932 R20033 N06002 N06007 N06022 N06030 N06059 N06200 N06230 N06455 N06686 N06975 N06985 N08031 N08320 N10001 N10276 N10624 N10629 N10665 N10675 N12160 R20033 R30556 A96061 N08031
Product Form Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Tread Plate Bar & Wire
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 649 B 649 B 649 B 649 B 658 B 658 B 658 B 668 B 672 B 673 B 673 B 673 B 674 B 674 B 674 B 675 B 675 B 676 B 676 B 677 B 677 B 677 B 686 B 688 B 688 B 690 B 690 B 691 B 691 B 704 B 704 B 705 B 705 B 709 B 710 B 710 B 718 B 719 B 720 B 722 B 723 B 726 B 755 B 756
Type, Grade, or Alloy Designation
Material UNS Number Number
Fe-Ni-Cr-Mo (Alloy 904L) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 1925) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 926) Cr-Fe-Ni-Mo (Alloy 33) R60702 R60704 R60705 Ni-Fe-Cr-Mo-Cu (Alloy 28) Fe-Ni-Cr-Mo-Cb (Alloy 700) Fe-Ni-Cr-Mo (Alloy 904L) Fe-Ni-Cr-Mo-Cu-N (Alloy 1925) Fe-Ni-Cr-Cu (Alloy 926) Fe-Ni-Cr-Mo (Alloy 904L) Fe-Ni-Cr-Mo-Cu-N (Alloy 1925) Fe-Ni-Cr-Cu (Alloy 926) Fe-Ni-Cr-Mo Fe-Ni-Cr-Mo (Alloy AL-6XN) Fe-Ni-Cr-Mo Fe-Ni-Cr-Mo (Alloy AL-6XN) Fe-Ni-Cr-Mo (Alloy 904L) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 1925) Fe-Ni-Cr-Mo-Cu-(Lo C) (Alloy 926) A356.0 (T61) Fe-Ni-Cr-Mo Fe-Ni-Cr-Mo (Alloy AL-6XN) Fe-Ni-Cr-Mo Fe-Ni-Cr-Mo (Alloy AL-6XN) Fe-Ni-Cr-Mo Fe-Ni-Cr-Mo (Alloy AL-6XN) Ni-Cr-Mo-Cb (Alloy 625) Ni-Fe-Cr-Mo-Cu-Ti (Alloy 825) Ni-Cr-Mo-Cb (Alloy 625) Ni-Fe-Cr-Mo-Cu-Ti (Alloy 825) Ni-Fe-Cr-Mo-Cu (Alloy 28) Ni-Fe-Cr-Si (Alloy 330) Ni-Fe-Cr-Si (Alloy 330TX) Ni-Cr-Mo-Co-W-Si (Alloy 333) Ni-Cr-Mo-Co-W-Si (Alloy 333) Fe-Cr-Ni-Mo Ni-Cr-Mo-Co-W-Si (Alloy 333) Ni-Cr-Mo-Co-W-Si (Alloy 333) Ni-Cr-Mo-Co-W-Si (Alloy 333) Ni-Cr-Mo-W Ni-Cr-Mo-W
45 45 45 45 61 61 62 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 26 45 45 45 45 45 45 43 45 43 45 45 45 45 45 45 45 45 45 45 43 43
(Continued)
63
N08904 N08925 N08926 R20033 R60702 R60704 R60705 N08028 N08700 N08904 N08925 N08926 N08904 N08925 N08926 N08366 N08367 N08366 N08367 N08904 N08925 N08926 A13560 N08366 N08367 N08366 N08367 N08366 N08367 N06625 N08825 N06625 N08825 N08028 N08330 N08332 N06333 N06333 N08310 N06333 N06333 N06333 N06110 N06110
Product Form Bar & Wire Bar & Wire Bar & Wire Bar & Wire Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless Tube Bar Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Welded Pipe Welded Pipe Welded Tube Welded Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Investment Castings Plate, Sheet & Strip Plate, Sheet & Strip Seamless Pipe & Tube Seamless Pipe & Tube Round & Square Rods & Bars Round & Square Rods & Bars Welded Tube Welded Tube Welded Pipe Welded Pipe Plate, Sheet & Strip Welded Pipe Welded Pipe Plate, Sheet & Strip Bars Seamless Tube Seamless Pipe & Tube Welded Pipe Welded Tube Plate, Sheet & Strip Rod & Bar
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 757 B 758 B 759 B 804 B 819 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862
Type, Grade, or Alloy Designation
Material UNS Number Number
Ni-Cr-Mo-W Ni-Cr-Mo-W Ni-Cr-Mo-W Alloy AL-6XN Deoxidized High P Cu (DHP) Grade 1 Grade 2 Grade 3 Grade 5 Grade 7 Grade 9 Grade 11 Grade 12 Grade 13 Grade 14 Grade 15 Grade 16 Grade 17 Grade 18 Grade 19 Grade 20 Grade 21 Grade 23 Grade 24 Grade 25 Grade 28 Grade 29 Grade 33 Grade 34 Grade 35 Grade 1 Grade 2 Grade 3 Grade 5 Grade 7 Grade 9 Grade 11 Grade 12 Grade 13 Grade 14 Grade 15 Grade 16 Grade 17 Grade 18
43 43 43 45 31 51 51 52 54 51 53 51 52 51 52 52 51 51 53 53 53 53 54 54 54 53 54 51 52 54 51 51 52 54 51 53 51 52 51 52 52 51 51 53 (Continued)
64
N06110 N06110 N06110 N08367 C12200 R50250 R50400 R50550 R56400 R52400 R56320 R52250 R53400 R53413 R53414 R53415 R52402 R52252 R56322 R58640 R58645 R58210 R56402 R56405 R56403 R56323 R56404 — — — R50250 R50400 R50550 R56400 R52400 R56320 R50250 R53400 R53413 R53414 R53415 R52402 R52252 R56322
Product Form Welded Pipe Welded Tube Pipe & Tube Welded Pipe & Tube Seamless Tube Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
AWS B2.1/B2.1M-BMG:2009
Table D.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys Base Metal Standard Specification
Type, Grade, or Alloy Designation
Material UNS Number Number
Product Form
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862 B 862
Grade 19 Grade 20 Grade 21 Grade 23 Grade 24 Grade 25 Grade 26 Grade 27 Grade 28 Grade 29 Grade 33 Grade 34 Grade 35
53 53 53 54 54 54 51 51 53 54 51 52 54
R58640 R58645 R58210 R56402 R56405 R56403 R52404 R52254 R56323 R56404 — — —
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
AMS AMS AMS AMS AMS AMS AMS
4914 4915 4919 4973 4975 4976 5711
15-3 8Al-1 Mo-1 V Al-Zr-Mo-Sn Al-Mo-V Al-Zr-Mo-Sn Al-Zr-Mo-Sn Ni-Cr-Mo
53 54 54 54 54 54 44
R58153 R54810 R54620 R54810 R54620 R54620 N06635
Sheet (Solution Treated) Sheet, Strip & Plate (Single Annealed) Sheet (Duplex Annealed) Forgings (Solution Treated & Stabilized) Bar (Solution Treated, Duplex Annealed) Forging, STA (Duplex Annealed) Sheet
ISO ISO
209 209
7020 (T5) 6082 (T4, T6)
27 23
A97020 A96082
Ext. Bar, Rod, Wire, Shapes & Tube Ext. Rod, Bar, Shapes & Tube
MR-01-75
Ni-Cr-Fe-Mo
45
N06950
Pipe
NACE
65
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
A 31 A 36 A 36 A 36 A 36 A 36 A 36 A 36 A 53 A 53 A 53 A 53 A 53 A 106 A 106 A 108 A 108 A 108 A 131 A 131 A 131 A 131 A 131 A 131 A 131 A 134 A 134 A 134 A 134
Grade B A36 A36 A36 A36 A36 A36 A36 Type E, Grade A Type E, Grade B Type F, Grade A Type S, Grade A Type S, Grade B Grade A Grade B Grade 1015 CW Grade 1018 CW Grade 1020 CW Grade A Grade A Grade B Grade D Grade E Grade CS Grade DS A36 A283 A A283 B A283 C
K03100 K02599 K02598 K02597 K02596 K02595 K02595 K02600 K02504 K03005 — K02504 K03005 K02501 K03006 G10150 G10180 G10200 K02300 K02300 K02102 K02101 K01801 K01601 K01601 — — — K02401
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
58/29 [400/200] 58/36 [400/248] 58/36 [400/248] 58/36 [400/248] 58/36 [400/248] 58/36 [400/248] 58/32 [400/221] 58/36 [400/248] 48/30 [331/207] 60/35 [414/241] 48/30 [331/207] 48/30 [331/207] 60/35 [414/241] 48/30 [331/207] 60/35 [414/241] 43/25 [296/172] 43/25 [296/172] 43/25 [296/172] 58/34 [400/234] 58/32 [400/221] 58/34 [400/234] 58/34 [400/234] 58/34 [400/234] 58/34 [400/234] 58/34 [400/234] 58/36 [400/248] 45/24 [310/165] 50/27 [345/186] 55/30 [379/207]
Rivets Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate Shapes Resistance Welded Pipe Resistance Welded Pipe Furnace Welded Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Bar Bar Bar Structural Structural Structural Structural Structural Structural Structural Welded Pipe Welded Pipe Welded Pipe Welded Pipe
C C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C C-Mn C C C-Mn C-Mn C-Mn C C C C C C C-Si C-Si C-Si C-Si C C C C
Steel and Steel Alloys
66
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
— ≤0.75 [19] >0.75 ≤1.5 [>19 ≤38] >1.5 ≤2.5 [>38 ≤64] >2.5 ≤4.0 [>64 ≤100] >4.0 ≤8.0 [>100 ≤200] >8.00 [200] ≤4.0 [100] — — — — — — — — — — ≤1.0 [25] >1.0 [25] — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
60/33 [414/228] 45/24 [310/165] 50/27 [345/186] 55/30 [379/207] 48/30 [331/207] 60/35 [414/241] 48/30 [331/207] 60/35 [414/241] 60/42 [414/290] 60/46 [414/317] 47/26 [324/179] 47/26 [324/179] 60/37 [414/255] 47/26 [324/179] 60/30 [414/207] 47/26 [324/179] 60/37 [414/255] 47/26 [324/179] 60/30 [414/207] 47/26 [324/179] 60/35 [414/241] 50/30 [345/207] 60/35 [414/241] 66/45 [455/310] 60/30 [414/207] 45/24 [310/165] 50/27 [345/186] 55/30 [379/207] 60/33 [414/228]
Welded Pipe Welded Pipe Welded Pipe Welded Pipe ERW Pipe ERW Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Low C Tube ERW Tube ERW Tube Seamless Tube Pipe Flanges Seamless Tube Seamless Tube ERW Tube Castings ERW Tube Pipe Fittings Pipe Piles Pipe Piles Pipe Piles Seamless Forging Plate Plate Plate Plate
C C C C C C-Mn C-Mn C-Mn C-Mn C-Mn C C C C C-Si C-Si C-Si C C-Si C-Si C-Si C C C C-Si C C C C
Steel and Steel Alloys
67
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 134 A 134 A 134 A 134 A 135 A 135 A 139 A 139 A 139 A 139 A 161 A 178 A 178 A 179 A 181 A 192 A 210 A 214 A 216 A 226 A 234 A 252 A 252 A 252 A 266 A 283 A 283 A 283 A 283
A283 D A285 A A285 B A285 C Grade A Grade B Grade A Grade B Grade C Grade D Low Carbon Grade A Grade C — Class 60 — Grade A1 — Grade WCA — Grade WPB Grade 1 Grade 2 Grade 3 Grade 1 Grade A Grade B Grade C Grade D
K02702 K01700 K02200 K02801 — — — K03003 K03004 K03010 K01504 K01200 K03503 K01200 K03502 K01201 K02707 K01807 J02502 K01201 K03006 — — — K03506 K01804 K02001 K02401 K02702
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
45/24 [310/165] 50/27 [345/186] 55/30 [379/207] 55/30 [379/207] 60/35 [414/241] 55/30 [379/207] 60/35 [414/241] 60/30 [414/207] 60/30 [414/207] 65/35 [448/241] 43/20 [296/138] 48/30 [331/207] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/42 [414/290] 63/46 [434/317] 62/48 [427/331] 45/25 [310/172] 50/30 [345/207] 55/33 [379/228] 60/35 [414/241] 65/38 [448/262] 60/35 [414/241] 45/33 [310/228] 58/42 [400/290] 62/46 [427/317] 58/36 [400/248] 40/20 [276/138]
Plate Plate Plate Seamless & Welded Pipe Seamless & Welded Pipe Welded Tube Welded Tube Forging Castings Castings Sheet Forging Forging Forging Pipe Pipe Pipe Pipe Sheet Sheet Sheet Sheet Sheet Pipe Fittings Tube Tube Tube Tube Mechanical Tube
C C C C-Mn C-Mn-Si C-Mn C-Mn-Si C-Mn-Si C-Si C-Si C C-Si C-Mn C-Si C-Mn C-Mn C-Mn C-Mn C C C C-Mn C-Mn C-Mn-Si C C C C C
Steel and Steel Alloys
68
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 285 A 285 A 285 A 333 A 333 A 334 A 334 A 350 A 352 A 352 A 366 A 369 A 369 A 372 A 381 A 381 A 381 A 381 A 414 A 414 A 414 A 414 A 414 A 420 A 500 A 500 A 500 A 501 A 512
Grade A Grade B Grade C Grade 1 Grade 6 Grade 1 Grade 6 Grade LF1 Grade LCA Grade LCB Commercial Quality Grade FPA Grade FPB Grade A Class Y35 Class Y42 Class Y46 Class Y48 Grade A Grade B Grade C Grade D Grade E Grade WPL6 Grade A round Grade B round Grade C round — Grade 1010
K01700 K02200 K02801 K03008 K03006 K03008 K03006 K03009 J02504 J03003 — K02501 K03006 K03002 K03013 — — — K01501 K02201 K02503 K02505 K02704 — K03000 K03000 K02705 K03000 G10100
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
40/20 [276/138] 40/20 [276/138] 43/25 [296/172] 50/30 [345/207] 55/35 [379/241] 40/20 [276/138] 43/25 [296/172] 50/30 [345/207] 40/20 [276/138] 50/30 [345/207] 65/55 [448/379] 42/30 [290/207] 45/32 [310/221] 48/35 [331/241] 48/35 [331/241] 48/35 [331/241] 48/35 [331/241] 52/38 [359/262] 54/40 [372/276] 56/40 [386/276] 55/30 [379/207] 60/32 [414/221] 65/35 [448/241] 55/30 [379/207] 60/32 [414/221] 65/35 [448/241] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138]
Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Plate Plate Plate Plate Plate Plate Mechanical Tube Mechanical Tube Mechanical Tube
C C C C C C C C C C C C C C C C C C C C C-Si C-Si C-Si C-Mn-Si C-Mn-Si C-Mn-Si C C C
Steel and Steel Alloys
69
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 512 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 513 A 515 A 515 A 515 A 516 A 516 A 516 A 519 A 519 A 519
Grade 1015 Grade 1117 Grade 1018 Grade 1020 Grade 1025 Grade MT1010 Grade MT1015 Grade MT1020 Grade MTX1015 Grade MTX1020 Grade 1015 CW Grade 1008 Grade 1010 Grade 1015 Grade 1017 Grade 1018 Grade 1019 Grade 1020 Grade 1021 Grade 1025 Grade 55 Grade 60 Grade 65 Grade 55 Grade 60 Grade 65 Grade 1008 Grade 1012 Grade 1016
G10150 G11170 G10180 G10200 G10250 G10100 G10150 G10200 — — G10150 G10080 G10100 G10150 G10170 G10180 G10190 G10200 G10210 G10250 K02001 K02401 K02800 K01800 K02100 K02403 G10080 G10120 G10160
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
40/20 [276/138] 43/25 [296/172] 43/25 [296/172] 50/30 [345/207] 50/30 [345/207] 50/32 [345/221] 50/30 [345/207] 50/30 [345/207] 50/30 [345/207] 55/35 [379/241] 55/35 [379/241] 55/35 [379/241] 55/35 [379/241] 40/20 [276/138] 43/25 [296/172] 50/30 [345/207] 40/20 [276/138] 60/30 [414/207] 66/33 [455/228] 48/30 [331/207] 60/35 [414/241] 60/35 [414/241] 55/30 [379/207] 42/25 [290/172] 42/25 [290/172] 60/42 [414/290] 45/35 [310/241] 47/26 [324/179] 60/37 [414/255]
Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Mechanical Tube Die Forging Die Forging Pipe Pipe Pipe Pipe Galvanized Sheet Galvanized Sheet Structural Coiled Tube Seamless Tube Seamless Tube
C C C C C C C C C C C C C C C C C C C C-Mn C-Mn C-Mn-Si C-Mn-Si — — 1.35maxMn-0.27maxC C C C-Si
Steel and Steel Alloys
70
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 519 A 521 A 521 A 523 A 523 A 524 A 524 A 526 A 527 A 529 A 539 A 556 A 556
Grade 1017 Grade 1018 Grade 1018 HR Grade 1019 Grade 1020 Grade 1020 HR Grade 1021 Grade 1022 Grade 1022 HR Grade 1025 Grade 1025 HR Grade 1026 Grade 1026 HR Grade MT1010 Grade MT1015 Grade MT1020 Grade MTX1015 Class CC Class CCI Grade A Grade B Grade I Grade II Grade II Grade II Grade 42 — Grade A2 Grade B2
G10170 G10180 G10180 G10190 G10200 G10200 G10210 G10220 G10220 G10250 G10250 G10260 G10260 G10100 G10150 G10200 G10150 — — K02504 K03005 K02104 K02104 K02104 K02104 K02703 K01506 K01807 K02707
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
47/26 [324/179] 60/37 [414/255] 55/30 [379/207] 49/30 [338/207] 52/33 [359/228] 53/36 [365/248] 53/40 [365/276] 60/45 [414/310] 65/50 [448/345] 49/30 [338/207] 52/33 [359/228] 53/36 [365/248] 55/40 [379/276] 60/45 [414/310] 65/50 [448/345] 70/55 [483/379] 60/42 [414/290] 60/42 [414/290] 65/50 [448/345] 65/50 [448/345] 58/32 [400/221] 65/35 [448/241] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 50/30 [345/207] 55/35 [379/241]
Tube-RW Tube-RW Plate Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Plate & Bars Shapes Plate & Bars Shapes Plate Plate Bar Bar Bar Bar Bar Bar Bar
C C C-Mn-Ti C C C C C C C C C C C C C C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C C C C C C C
Steel and Steel Alloys
71
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 557 A 557 A 562 A 569 A 569 A 569 A 569 A 569 A 569 A 570 A 570 A 570 A 570 A 570 A 570 A 570 A 572 A 572 A 572 A 572 A 573 A 573 A 575 A 575 A 575 A 575 A 575 A 575 A 575
Grade A2 Grade B2 — Grade 30 Grade 33 Grade 36 Grade 40 Grade 45 Grade 50 Grade 30 Grade 33 Grade 36 Grade 40 Grade 45 Grade 50 Grade 55 Grade 42 Grade 42 Grade 50 Grade 50 Grade 58 Grade 65 Grade M1008 Grade M1010 Grade M1012 Grade M1015 Grade M1017 Grade M1020 Grade M1023
K01807 K03007 K11224 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02502 K02303 K02303 K02304 K02304 K02301 K02404 G10080 G10100 G10120 G10150 G10170 G10200 G10230
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
55/35 [379/241] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 45/25 [310/172] 45/25 [310/172] 50/30 [345/207] 50/30 [345/207] 50/30 [345/207] 55/35 [379/241] 55/35 [379/241] 48/30 [331/207] 47/26 [324/179] 60/37 [414/255] 65/45 [448/310] 65/50 [448/345] 42/25 [290/172] 45/30 [310/207] 48/33 [331/228] 52/40 [359/276] 65/50 [448/345] 40/22 [276/152] 40/22 [276/152] 63/42 [434/290] 45/33 [310/228] 52/37 [359/255]
Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Bar Pipe Tube-RW Tube-RW Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Tube Sheet Sheet Plate & Shapes Galvanized Sheet Galvanized Sheet
C C C C C C C C C C C C C C C C C C-Mn-Cb-V C-Mn-Cb-V C-Mn C-Mn C-Mn C-Mn Mn-V C C Mn-Cb — —
Steel and Steel Alloys
72
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 575 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 576 A 587 A 587 A 587 A 607 A 607 A 611 A 611 A 611 A 611 A 618 A 620 A 620 A 633 A 653 A 653
Grade M1025 Grade 1008 Grade 1010 Grade 1012 Grade 1015 Grade 1016 Grade 1017 Grade 1018 Grade 1019 Grade 1020 Grade 1021 Grade 1022 Grade 1023 Grade 1025 — Grade A2 Grade B2 Grade 45 Grade 50 Grade A Grade B Grade C Grade D Grade III Types A Types B Grade A Grade 33 Grade 37
G10250 G10080 G10100 G10120 G10150 G10160 G10170 G10180 G10190 G10200 G10210 G10220 G10230 G10250 K11500 K01807 K03007 — — G10170 G10170 G10170 G10120 K12700 K00040 K00040 K01802 — —
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
73
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 653 A 653 A 656 A 656 A 660 A 662 A 662 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 663 A 668 A 668 A 671 A 671 A 671 A 671 A 671 A 672 A 672 A 672 A 672 A 672
Grade 40 Grade 80 Grade 50 Grade 60 Grade WCA Grade A Grade B Grade 45 Grade 45 Grade 50 Grade 50 Grade 55 Grade 55 Grade 60 Grade 60 Grade 65 Grade 65 Class B Class C Grade CA55 Grade CB60 Grade CB65 Grade CC60 Grade CC65 Grade A45 Grade A50 Grade A55 Grade B60 Grade B65
— — K11804 K11804 J02504 K01701 K02203 — — — — — — — — — — G10200 G10250 K02801 K02401 K02800 K02100 K02403 K01700 K02200 K02801 K02401 K02800
— — ≤2 [50] ≤1.5 [38] — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
55/40 [379/276] 82/80 [565/552] 60/50 [414/345] 70/60 [483/414] 60/30 [414/207] 58/40 [400/276] 65/40 [448/276] 45/25 [310/172] 45/25 [310/172] 50/28 [345/193] 50/28 [345/193] 55/30 [379/207] 55/30 [379/207] 60/33 [414/228] 60/33 [414/228] 65/36 [448/248] 65/36 [448/248] 60/30 [414/207] 66/30 [455/207] 55/30 [379/207] 60/32 [414/221] 65/35 [448/241] 60/32 [414/221] 65/35 [448/241] 45/24 [310/165] 50/27 [345/186] 55/30 [379/207] 60/32 [414/221] 65/35 [448/241]
Galvanized Sheet — Galvanized Sheet — Hi-Str. Lo-Alloy Plate 1.65maxMn-0.6Si-0.18maxC Hi-Str. Lo-Alloy Plate 1.65maxMn-0.6Si-0.18maxC Centrifugal Cast Pipe C Plate C-Mn-Si Plate C-Mn-Si Bar C Shapes, Rounds, Squares, Hex. C Bar C Shapes, Rounds, Squares, Hex. C Bar C Shapes, Rounds, Squares, Hex. C Bar C Shapes, Rounds, Squares, Hex. C Bar C Shapes, Rounds, Squares, Hex. C Forging C Forging C Fusion Welded Pipe C Fusion Welded Pipe C-Mn-Si Fusion Welded Pipe C-Mn-Si Fusion Welded Pipe C-Mn-Si Fusion Welded Pipe C-Mn-Si Fusion Welded Pipe C Fusion Welded Pipe C Fusion Welded Pipe C Fusion Welded Pipe C-Si Fusion Welded Pipe C-Si
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Bar Bar Bar Bar Bar Bar Bar Forging Forging Forging Forging Forging Plate, Bars & Shapes Plate, Bars & Shapes Forging Forging Resistance Welded Pipe Resistance Welded Pipe Seamless Pipe Seamless Pipe Furnace-Welded Pipe Structural Structural Structural Plate
C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C C C C C C-Mn-Si C-Mn-Si C-1Mn C-1Mn 1.3Mn-V 1.8Ni-0.55Mn-0.25Mo 1.2Cu-0.9Ni-0.7Cr-0.5Mn C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn C-Mn C-Mn — C-Mn-Si-Cb-W C-Mn-Si-Cb-W C-Mn-Si-Cb-W C
Steel and Steel Alloys
74
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM/AISI
A 672 A 672 A 672 A 672 A 675 A 675 A 675 A 675 A 675 A 695 A 696 A 707 A 707 A 707 A 707 A 707 A 709 A 709 A 727 A 765 A 795 A 795 A 795 A 795 A 795 A 808 A 808 A 808 A 830
Grade C55 Grade C60 Grade C65 Grade E60 Grade 45 Grade 50 Grade 55 Grade 60 Grade 65 Type B Grade B Grade L1, Class 1 Grade L2, Class 1 Grade L3, Class 1 Grade L4, Class 1 Grade L5, Class 1 Grade 36 Grade 50 Grade 36 Grade I 1 Type, Grade B Type E, Grade A Type S, Grade A Type S, Grade B Type F — — — 1006
K01800 — 55/30 [379/207] K02100 — 60/32 [414/221] K02403 — 65/35 [448/241] K02402 — 60/32 [414/221] — — 45/22.5 [310/155] — — 50/25 [345/172] — — 55/27.5 [379/190] — — 60/30 [414/207] — — 65/32.5 [448/224] K03504 — 60/35 [414/241] K03200 — 60/35 [414/241] K02302 — 60/42 [414/290] K03301 — 60/42 [414/290] K12510 — 60/42 [414/290] K12089 — 60/42 [414/290] K20934 — 60/42 [414/290] — — 58/36 [400/248] — — 65/50 [448/345] K02506 — 60/36 [414/248] K03046 — 60/30 [414/207] — — 60/– [414/–] — — 60/– [414/–] — — 60/– [414/–] — — 60/– [414/–] — — 60/– [414/–] K11852 ≤1.5 [38] 65/50 [448/345] K11852 >1.5 ≤2.0 [>38 ≤50] 65/46 [448/317] K11852 >2.0 ≤2.5 [>50 ≤64] 60/42 [414/290] G10060 — 40/20 [276/138] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
75
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM/AISI ASTM ASTM
A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 830 A 836 A 857
1008 1009 1010 1012 1015 1016 1017 1018 1019 1020 1021 1022 1023 1025 Class 1 Grade 25
G10080 G10090 G10100 G10120 G10150 G10160 G10170 G10180 G10190 G10200 G10210 G10220 G10230 G10250 — —
— — — — — — — — — — — — — — — —
40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 40/20 [276/138] 43/25 [296/172] 43/25 [296/172] 43/25 [296/172] 43/25 [296/172] 43/25 [296/172] 43/25 [296/172] 50/30 [345/207] 55/25 [379/172] 38/25 [262/172]
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Forging Sheet Piling
1
1
ASTM
A 857
Grade 30
—
—
49/30 [338/207]
Sheet Piling
1
1
ASTM
A 857
Grade 33
—
—
52/33 [359/228]
Sheet Piling
1
1
ASTM
A 857
Grade 36
—
—
53/36 [365/248]
Sheet Piling
1 1 1 1 1 1
1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM
A 935 A 935 A 935 A 935 A 984 A 992
Grade 45, Class 1 Grade 45, Class 2 Grade 50, Class 1 Grade 50, Class 2 Grade 35 —
— — — — — —
— — — — — —
65/45 [448/310] 55/45 [379/310] 65/50 [448/345] 60/50 [414/345] 60/35 [414/241] 65/50 [448/345]
Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Line Pipe Structural Shapes
(Continued)
C C C C C C C C C C C C C C C-Si-Ti 1.5maxMn-0.35max P-0.25maxC-0.2minCu 1.5maxMn-0.35max P-0.25maxC-0.2minCu 1.5maxMn-0.35max P-0.25maxC-0.2minCu 1.5maxMn-0.35max P-0.25maxC-0.2minCu C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C C-Mn-Si
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
— — — — — — — — — — — — — — —
— — — — — — — — — — — — — — —
Sheet Sheet Sheet Sheet Sheet Sheet Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip
— — — — — — — — — — — — — — —
—
—
Sheet & Strip
—
—
—
Sheet & Strip
—
—
—
Sheet & Strip
—
—
—
Sheet & Strip
—
—
58/34 [400/234]
Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel
C
Steel and Steel Alloys
76
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 1008 A 1008 A 1008 A 1008 A 1008 A 1008 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011 A 1011
CS Type B — DS Type B — SS Grade 25 — SS Grade 30 — SS Grade 33 Type 1, 2 — SS Grade 40 Type 1, 2 — CS Type B — DS Type B — SS Grade 30 — SS Grade 33 — SS Grade 36 — SS Grade 40 — SS Grade 45 — SS Grade 50 — HSLAS Grade 45 — Class 1 HSLAS Grade 45 — Class 2 HSLAS Grade 50 — Class 1 HSLAS Grade 50 — Class 2 HSLAS Grade 55 — Class 2 Grade A K02300
1
1
ASTM
A 1011
1
1
ASTM
A 1011
1
1
ASTM
A 1011
1
1
ASTM
A 1011
1
1
ABS
ABS
1
1
ABS
ABS
Grade B
K02102
—
58/34 [400/234]
1
1
ABS
ABS
Grade D
K02101
—
58/34 [400/234]
(Continued)
C C-Si
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
77
1
ABS
ABS
Grade E
K01801
—
58/34 [400/234]
1
1
ABS
ABS
Grade AH32
K11846
—
64/46 [441/317]
1
1
ABS
ABS
Grade DH32
K11846
—
64/46 [441/317]
1
1
ABS
ABS
Grade EH32
K11846
—
64/46 [441/317]
1
1
ABS
ABS
Grade FH32
K11846
—
64/46 [441/317]
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
API API API API API API API API API AS AS AS AS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS
2H 5L 5L 5L 5L 5L 5LS 2Y 2Y 1548 1548 1548 1548 3678 3678 3678 3678 3678 3678
Grade 42 Grade A25, Class I Grade A25, Class II Grade A Grade B Grade 42 Grade X46 Grade X42 Grade 50 7-430 7-430 7-430 7-430 200 250 250 250 250 250
— — — — — — — — — — — — — — — — — — —
— — — — — — — — — ≤0.625 [16] >0.625 ≤1.56 [>16 ≤40] >1.56 ≤3.125 [>40 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.5 [13] ≤0.31 [8] >0.31 ≤0.5 [>8 ≤13] >0.5 ≤2 [>13 ≤50] >2 ≤3.125 [50 ≤78] >3.125 ≤6 [>78 ≤150]
62/42 [427/290] 45/25 [310/172] 45/25 [310/172] 48/30 [331/207] 60/35 [414/241] 60/42 [414/290] 63/46 [434/317] 62/42 [427/290] 65/50 [448/345] 62/44 [427/303] 62/41 [427/283] 62/39 [427/269] 62/36 [427/248] 44/29 [303/200 60/41 [414/283] 60/38 [414/262] 60/36 [414/248] 60/35 [414/241] 60/33 [414/228]
(Continued)
Ordinary Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel Structural Pipe & Tube Pipe & Tube Pipe Pipe Pipe Pipe Pipe Pipe Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate
C-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C C C C C C-Mn C-Mn C-Mn C-Mn C-Mn
AWS B2.1/B2.1M-BMG:2009
1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Plate Plate Plate Plate Plate Flats & Sections Flats & Sections Flats & Sections Flats & Sections Hex, Squares & Rounds Hex, Squares & Rounds Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Strip Structural Structural
C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C C C C C C-Mn C C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn-Cr-Ni-Cu C-Mn C-Mn C-Mn C C
Steel and Steel Alloys
78
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS CSA CSA
3678 3678 3678 3678 3678 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 1594 G40.20/40.21 G40.20/40.21
250L15 250L15 250L15 250L15 250L15 250/250L0/250L15 250/250L0/250L15 250/250L0/250L15 250/250L0/250L15 250/250L0/250L15 250/250L0/250L15 HA1 HA3 HA4N HA200 HA250 HU250 HA250/1 HA300 HU300 HA300/1 HU300/1 HA350 HW350 HA400 XF300 XF400 260W 260WT
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
≤0.31 [8] 60/41 [414/283] >0.31 ≤0.5 [>8 ≤13] 60/38 [414/262] >0.5 ≤2 [>13 ≤50] 60/36 [414/248] >2 ≤3.125 [>50 ≤78] 60/35 [414/241] >3.125 ≤6 [>78 ≤150] 60/35 [414/241] <0.44 [11] 60/38 [414/262] ≥0.44 <0.625 [≥11 <16] 60/36 [414/248] ≥0.625 <1.56 [≥16 <40] 60/36 [414/248] ≥1.56 [40] 60/33 [414/228] ≤2 [50] 60/36 [414/248] >2 ≥4 [>50 ≥100] 60/33 [414/228] — 44/29 [303/200] — 44/29 [303/200] — 41/25 [283/172] — 44/29 [303/200] — 51/36 [352/248] — 51/36 [352/248] — 50/36 [345/248] — 58/44 [400/303] — 58/44 [400/303] — 62/44 [427/303] — 62/44 [427/303] — 62.3/51 [429/352] — 65/49 [448/338] — 67/55 [462/379] — 64/44 [441/303] — 67/55 [462/379] — 60/38 [414/262] — 60/38 [414/262] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
65/44 [448/303] 65/44 [448/303] 45/25 [310/172] 48/30 [331/207] 60/35 [414/241] 60/42 [414/290] 48/30 [331/207] 60/35 [414/241] 60/42 [414/290] 60/36 [414/248] 60/42 [414/290] 60/42 [414/290] 63/46 [434/317] 66/52 [455/359]
Structural Structural Pipe Pipe Pipe Pipe Steel Fittings Steel Fittings Steel Fittings Steel Flanges Steel Flanges Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings
C-Mn-Cb-V C-Mn-Cb-V C C C C C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn C-Mn
70/36 [483/248] 70/40 [483/276] 64/46 [441/317] 71/51 [490/352] 64/46 [441/317] 71/51 [490/352] 64/46 [441/317] 71/51 [490/352] 66/52 [455/359] 70/40 [483/276] 70/36 [483/248] 70/40 [483/276] 70/36 [483/248] 70/40 [483/276]
Pipe Flanges Seamless Pipe Structural Structural Structural Structural Structural Structural Welded Pipe ERW Tube Pipe Flanges ERW Tube Castings Castings
C-Mn C-Mn C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn C-Si C-Mn C-Si C-Mn-Si
Steel and Steel Alloys
79
1 1 1 1 1 1 1 1 1 1 1 1 1 1
CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA MSS MSS MSS
G40.20/40.21 G40.20/40.21 Z245.1 Z245.1 Z245.1 Z245.1 Z245.11 Z245.11 Z245.11 Z245.12 Z245.12 SP75 SP75 SP75
300W 300WT 172 207 241 290 207 241 290 248 290 WPHY-42 WPHY-46 WPHY-52
— — — — — — — — — — — — — —
1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 105 A 106 A 131 A 131 A 131 A 131 A 131 A 131 A 139 A 178 A 181 A 210 A 216 A 216
— Grade C Grade AH32 Grade AH36 Grade DH32 Grade DH36 Grade EH32 Grade EH36 Grade E Grade D Class 70 Grade C Grade WCB Grade WCC
K03504 K03501 K11846 K11852 K11846 K11852 K11846 K11852 K03012 — K03502 K03501 J03002 J02503
— — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Pipe Fittings Shapes, Plates & Bars Shapes, Plates & Bars Shapes, Plates & Bars Seamless Forging Seamless Forging Seamless Forging Plate Plate Forging Forging Forging Castings Forging Pipe Pipe Pipe Sheet Sheet Plate Plate
C-Si LowC-P-Cu LowC-P-Cu LowC-P-Cu C-Si C-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si 1.3Mn-Si-V-N 1.15Cu-0.85Ni-0.75Cr-0.5Mn C-Mn-Si C-Mn-Si C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn
Plate
C-Mn
Castings Forging Forging Mechanical Tube Mechanical Tube
Low-C-Mn-Ni C-Si C-Mn-Si C C
Steel and Steel Alloys
80
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 234 A 242 A 242 A 242 A 266 A 266 A 266 A 299 A 299 A 350 A 350 A 350 A 352 A 372 A 381 A 381 A 381 A 414 A 414 A 455 A 455
1
2
ASTM
A 455
1 1 1 1 1
2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM
A 487 A 508 A 508 A 512 A 513
Grade WPC Type 1 Type 1 Type 1 Grade 2 Grade 3 Grade 4 Grade A Grade A Grade LF2 Grade LF6, Class 1 Grade LF787, Class 2 Grade LCC Grade B Class Y50 Class Y52 Class Y56 Grade F Grade G — —
Grade 16A Grade 1 Grade 1A Grade 1030 Grade 1020 CW
K03501 — 70/40 [483/276] K11510 ≤3/4 [19] 70/50 [483/345] K11510 >3/4 ≤1.5 [>19 ≤38] 67/46 [462/317] K11510 >1.5 ≤4.0 [>38 ≤100] 63/42 [434/390] K03506 — 70/36 [483/248] K05001 — 75/37.5 [517/259] K03017 — 70/36 [483/248] K02803 ≤1.00 [25] 75/42 [517/290] K02803 >1.00 [25] 75/40 [517/276] K03011 — 70/36 [483/248] K12202 — 66/52 [455/359] — — 65/55 [448/379] J02505 — 70/40 [483/276] K04001 — 75/45 [417/310] — — 64/50 [441/345] — — 66/52 [455/359] — — 71/56 [490/386] K03102 — 70/42 [483/290] K03103 — 75/45 [417/310] K03300 ≤0.375 [10] 75/38 [517/262] K03300 >0.375 ≤0.580 73/37 [503/255] [>10 ≤15] K03300 >0.580 ≤0.750 70/35 [483/241] [>10 ≤19] J31200 — 70/40 [483/276] K13502 — 70/36 [483/248] K13502 — 70/36 [483/248] G10300 — 75/55 [517/379] G10200 — 62/45 [427/310] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
62/45 [427/310] 70/55 [483/379] 75/55 [517/379] 70/38 [483/262] 70/38 [483/262] 75/55 [517/379] 75/37 [517/255] 65/50 [448/345] 70/50 [483/345] 70/50 [483/345] 70/55 [483/379] 70/55 [483/379] 70/55 [483/379] 70/50 [483/345] 65/45 [448/310] 70/36 [483/248] 70/36 [483/248] 70/40 [483/276] 70/40 [483/276] 70/55 [483/379] 70/42 [483/290] 70/50 [483/345] 67/46 [462/317] 63/42 [434/290] 70/50 [483/345] 67/46 [462/317] 63/42 [434/290] 70/50 [483/345] 67/46 [462/317]
Mechanical Tube Mechanical Tube Mechanical Tube Plate Plate Mechanical Tube Forging Shapes Plates Bars Shapes Plates Bars Plate Plate Forging Forging Seamless Tube ERW Tube Plate & Shapes Improved Toughness Plate Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate & Bars Plate & Bars
C C C C-Si C-Mn-Si C C 1.35maxMn-0.27maxC 1.35maxMn-0.27maxC 1.35maxMn-0.27maxC 1.35maxMn-0.27maxC 1.35maxMn-0.27maxC 1.35maxMn-0.27maxC C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn-Si C-Mn-Si C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V
Steel and Steel Alloys
81
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 513 A 513 A 513 A 515 A 516 A 519 A 521 A 529 A 529 A 529 A 529 A 529 A 529 A 537 A 537 A 541 A 541 A 556 A 557 A 572 A 573 A 588 A 588 A 588 A 588 A 588 A 588 A 588 A 588
Grade 1025 CW Grade 1026 Grade 1030 Grade 70 Grade 70 Grade 1030 Class CE Grade 50 Grade 50 Grade 50 Grade 55 Grade 55 Grade 55 Class 1 Class 1 Grade 1 Grade 1A Grade C2 Grade C2 Grade 55 Grade 70 Grade A Grade A Grade A Grade B Grade B Grade B Grade C Grade C
G10250 G10260 G10300 K03101 K02700 G10300 — — — — — — — K02400 K02400 K03506 — K03006 K03505 — K02701 K11430 K11430 K11430 K12043 K12043 K12043 K11538 K11538
— — — — — — — ≤1.5 [38] <1.0 [25] <3.5 [89] ≤1.5 [38] <1.0 [25] <3.0 [75] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] — — — — — — ≤4 [100] >4.0 ≤5.0 [>100 ≤125] >5.0 ≤8.0 {>125 ≤200] ≤4 [100] >4.0 ≤5.0 [>100 ≤125] >5.0 ≤8.0 [>125 ≤200] ≤4 [100] >4.0 ≤5.0 [>100 ≤125] (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
63/42 [434/290] 70/50 [483/345] 67/46 [462/317] 63/42 [434/290] 70/50 [483/345] 65/55 [448/379] 70/60 [483/414] 65/45 [448/310] 70/50 [483/345] 65/45 [448/310] 60/45 [414/310] 70/50 [483/345] 67/46 [462/317] 70/50 [483/345] 67/46 [462/317] 70/50 [483/345] 70/50 [483/345] 70/50 [483/345] 65/46 [448/317] 70/50 [483/345] 65/46 [448/317] 80/70 [552/483] 70/36 [483/248] 70/40 [483/276] 70/43 [483/296] 75/37.5 [517/259] 70/38 [483/262] 70/38 [483/262] 70/50 [483/345]
Plate & Bars Plate & Bars Plate & Bars Plate & Bars Structural Shapes Tapered Tube Tapered Tube Hot Rolled Sheet & Strip Hot Rolled Sheet & Strip Cold Rolled Sheet & Strip Sheet & Strip HSLA Tube HSLA Tube HSLA Tube HSLA Tube Tube Tube HSLA Steel HSLA Steel HSLA Steel HSLA Steel Hi-Str. Lo-Alloy Plate Centrifugal Cast Pipe Centrifugal Cast Pipe Plate Forging Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe
C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-Cb C-Mn-Ni-Cu-Cr-Cb C-Mn-Ni-Cu-Cr-Cb C-Mn-Ni-Cu-Cr-Cb C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn-Cb-V C-Mn C-Mn C-Mn-Cu C-Mn-Cu Mn-Cu-V Mn-Cu-V C-Mn-Si-Cb C-Mn-Si-Cb C-Mn-Si C-Mn-Si 1.65maxMn-0.6Si-0.18maxC C-Si C-Si C-Mn-Si C-Mn C-Si C-Mn-Si C-Mn-Si
Steel and Steel Alloys
82
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 588 A 588 A 588 A 588 A 588 A 595 A 595 A 606 A 606 A 606 A 607 A 618 A 618 A 618 A 618 A 618 A 618 A 633 A 633 A 633 A 633 A 656 A 660 A 660 A 662 A 668 A 671 A 671 A 671
Grade C Grade K Grade K Grade K All Grades Grade A Grade B Annealed or Norm As Rolled As Rolled Grade 45 Grade 1a Grade 1a Grade 1b Grade 1b Grade II Grade II Grade C Grade C Grade D Grade D Grade 70 Grade WCB Grade WCC Grade C Class D Grade CB70 Grade CC70 Grade CD70
K11538 — — — — K02004 K02005 — — — — — — K02601 K02601 K12609 K12609 K12000 K12000 K12037 K12037 K11804 J03003 J02505 K02007 G10300 K03101 K02700 K02400
>5.0 ≤8.0 {>125 ≤200] ≤4 [100] >4.0 ≤5.0 [>100 ≤125] >5.0 ≤8.0 {>125 ≤200] — — — — — — ≤0.75 [19] >0.75 ≤1.5 [>19 ≤38] ≤0.75 [19] >0.75 ≤1.5 [>19 ≤38] ≤0.75 [19] >0.75 ≤1.5 [>19 ≤38] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] ≤1 [25] — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
83
2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 671 A 672 A 672 A 672 A 672 A 675 A 675 A 678
Grade CK75 Grade B70 Grade C70 Grade D70 Grade N75 Grade 70 Grade 75 Grade B
K02803 K03101 K02700 K02400 K02803 — — K02002
— — — — — — — ≤2.5 [64]
75/40 [517/276] 70/38 [483/262] 70/38 [483/262] 70/50 [483/345] 75/40 [517/276] 70/35 [483/241] 75/37.5 [517/259] 80/60 [552/414]
Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Bar Bar Structural Plate
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 678 A 690 A 691 A 691 A 695 A 696 A 707 A 707 A 707 A 707 A 707 A 707 A 709 A 737 A 738 A 765 A 913 A 935 A 935 A 935
Grade A — Grade CMSH-70 Grade CMS-75 Type B, Grade 40 Grade C Grade L1, Class 2 Grade L2, Class 2 Grade L3, Class 2 Grade L4, Class 3 Grade L4, Class 2 Grade L5, Class 2 Grade 50W Grade B Grade A Grade II Grade 50 Grade 55 Class 1 Grade 55, Class 2 Grade 60, Class 1
K01600 K12249 K02400 K02803 K03504 K03200 K02302 K03301 K12510 K12089 K12089 K20934 — K12001 K12447 K03047 — — — —
≤1.5 [38] ≤4 [100] — — — — — — — — — — — — — — — — — —
70/50 [483/345] 70/50 [483/345] 70/50 [483/345] 75/40 [517/276] 70/40 [483/276] 70/40 [483/276] 66/52 [455/359] 66/52 [455/359] 66/52 [455/359] 75/60 [517/414] 66/52 [455/359] 66/55 [455/379] 70/50 [483/345] 70/50 [483/345] 75/45 [417/310] 70/36 [483/248] 65/50 [448/345] 70/55 [483/379] 65/55 [448/379] 75/60 [517/414]
Structural Plate Marine Piling—Plate & Bar Fusion Welded Pipe Fusion Welded Pipe Bar Bar Forging Forging Forging Forging Forging Forging Plate, Bars & Shapes Plate Plate Forging Structural Sheet & Strip Sheet & Strip Sheet & Strip
(Continued)
C-Mn-Si C-Si C-Mn-Si C-Mn-Si C-Mn-Si C C 1.0Mn-0.33Si (>1.5=1.3Mn-0.33Si) 1.2Mn-0.33Si 0.75Mn-0.58Ni-0.12P C-Mn-Si C-Mn-Si C-Mn-Si C C-1Mn C-1Mn 1.3Mn-V-N 1.8Ni-0.55Mn-0.25Mo 1.8Ni-0.55Mn-0.25Mo 1.2Cu-0.9Ni-0.7Cr-0.5Mn C-Mn-Cr-Si C-Mn-Si-Cb C-Mn-Si C-Mn-Si C-Mn — C-Mn-Cb-V C-Mn-Cb-V
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
84
1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ABS
A 935 A 984 A 984 A 984 A 1011 A 1011 A 1011 ABS
Grade 60, Class 2 — Grade 45 — Grade 55 — Grade 65 — SS Grade 55 — HSLAS Grade 55 cl 1 — HSLAS Grade 60 cl 2 — Grade AH36 K11852
— — — — — — — —
70/60 [483/414] 65/45 [448/310] 70/55 [483/379] 75/65 [517/448] 70/55 [483/379] 70/55 [483/379] 70/60 [483/414] 71/51 [490/352]
1
2
ABS
ABS
Grade DH36
K11852
—
71/51 [490/352]
1
2
ABS
ABS
Grade EH36
K11852
—
71/51 [490/352]
1
2
ABS
ABS
Grade FH36
K11852
—
71/51 [490/352]
1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2
API API API API API AS AS AS AS AS AS AS AS AS
2H 5L 5L 5L 2Y 1548 1548 1548 1548 1548 1548 1548 1548 1548
Grade 50 Grade X52 Grade X56 Grade X60 Grade 50T 5-490 5-490 5-490 5-490 7-460 7-460 7-460 7-460 7-490
— — — — — — — — — — — — — —
— — — — — ≤0.625 [16] >0.625 ≤1.56 [>16 ≤40] >1.56 ≤3.125 [>40 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.625 [16] >0.625 ≤1.56 [>16 ≤40] >1.56 ≤3.125 [>40 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.625 [16]
70/50 [483/345] 66/52 [455/359] 71/56 [490/386] 75/60 [517/414] 70/50 [483/345] 71/52 [490/359] 71/49 [490/338] 71/48 [490/331] 71/46 [490/317] 67/44 [462/303] 67/43 [462/296] 67/40 [462/276] 67/38 [462/262] 71/46 [490/317]
(Continued)
Sheet & Strip Line Pipe Line Pipe Line Pipe Sheet & Strip Sheet & Strip Sheet & Strip High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel High Strength Hull Structural Steel Structural Pipe Pipe Pipe Pipe Plate Plate Plate Plate Plate Plate Plate Plate Plate
C-Mn-Cb-V C C C — — — C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn-Cb-V-Ti C-Mn-Cb-V-Ti — C C C C C C C C C
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
71/45 [490/310] 71/44 [490/303] 71/41 [490/283] 62/46 [427/317] 62/45 [427/310] 62/44 [427/303] 62/41 [427/283] 62/39 [427/269] 62/38 [427/262] 65/52 [448/359] 65/51 [448/352] 65/49 [448/338] 65/48 [448/331] 70/58 [483/400] 70/55 [483/379] 70/52 [483/359] 75/65 [517/448] 73/61 [503/421] 73/58 [503/400] 64/46 [441/317] 64/44 [441/303] 64/41 [441/283] 64/44 [441/303] 64/42 [441/290] 64/41 [441/283] 70/52 [483/359] 70/49 [483/338] 70/49 [483/338] 70/48 [483/331]
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate Flats & Sections Flats & Sections Flats & Sections Hex, Squares & Rounds Hex, Squares & Rounds Hex, Squares & Rounds Flats & Sections Flats & Sections Flats & Sections Flats & Sections
C C C C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn
Steel and Steel Alloys
85
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
AS AS AS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS
1548 1548 1548 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3678 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1
7-490 7-490 7-490 300/300L15 300/300L15 300/300L15 300/300L15 300/300L15 300/300L15 350/350L15 350/350L15 350/350L15 350/350L15 400/400L15 400/400L15 400/400L15 400/400L15 400/400L15 400/400L15 300/300L0/300L15 300/300L0/300L15 300/300L0/300L15 300/300L0/300L15 300/300L0/300L15 300/300L0/300L15 350/350L0/350L15 350/350L0/350L15 350/350L0/350L15 350/350L0/350L15
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
>0.625 ≤1.56 [>16 ≤40] >1.56 ≤3.125 [>40 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.31 [8] >0.31 ≤0.5 [>8 ≤13] >0.5 ≤0.75 [>13 ≤19] >0.75 ≤2 [>19 ≤50] >2 ≤3.125 [>50 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.5 [13] >0.5 ≤0.75 [>13 ≤19] >0.75 ≤3.125 [>19 ≤78] >3.125 ≤6 [>78 ≤150] ≤0.5 [13] >0.5 ≤0.75 [>13 ≤19] >0.75 ≤3.125 [>19 ≤78] ≤0.75 [19] >0.75 ≤1.25 [>19 ≤29] >1.25 ≤2 [>29 ≤50] <0.44 [11] ≥0.44 <0.625 [≥11 <16] ≥0.625 ≥1.56 [≥16 ≥40] ≤2 [50] >2 <4 [>50 <100] ≥4 [100] <0.44 [11] ≥0.44 <0.625 [≥11 <16] ≥0.625 <1.56 [≥16 <40] ≤1.56 [40] (Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/49 [483/338] 70/48 [483/331] 70/46 [483/317] 75/58 [517/400] 75/58 [517/400] 75/55 [517/379] 75/55 [517/379] 75/58 [517/400] 75/55 [517/379] 75/52 [517/359] 70/50 [483/345] 70/50 [483/345] 70/50 [483/345] 65/50 [448/345] 70/50 [483/345] 70/55 [483/379] 70/55 [483/379] 75/60 [517/414] 75/60 [517/414] 75/60 [517/414] 75/60 [517/414] 90/80 [621/552] 90/80 [621/552] 90/80 [621/552] 90/80 [621/552] 63/46 [434/317] 66/52 [455/359] 71/56 [490/386] 63/46 [434/317]
Hex, Squares & Rounds Hex, Squares & Rounds Hex, Squares & Rounds Flats & Sections Flats & Sections Flats & Sections Flats & Sections Hex, Squares & Rounds Hex, Squares & Rounds Hex, Squares & Rounds HSLA Steel HSLA Steel HSLA Steel Structural Structural Structural Structural HSLA Steel HSLA Steel HSLA Steel HSLA Steel Structural Steel Structural Steel Structural Steel Structural Steel Pipe Pipe Pipe Steel Fittings
C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn C-Mn C-Mn C-Mn-Si
Steel and Steel Alloys
86
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS AS/NZS CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA CSA
3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 3679.1 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 Z245.1 Z245.1 Z245.1 Z245.11
350/350L0/350L15 350/350L0/350L15 350/350L0/350L15 400/400L0/400L15 400/400L0/400L15 400/400L0/400L15 400/400L0/400L15 400/400L0/400L15 400/400L0/400L15 400/400L0/400L15 350A 350AT 350R 350W 350WT 380W 380WT 400A 400AT 400W 400WT 550A 550AT 550W 550WT 317 359 386 317
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
≤2 [50] >2 <4 [>50 <100] ≥4 [100] <0.44 [11] ≥0.44 <0.625 [≥11 <16] ≥0.625 <1.56 [≥16 <40] ≤1.56 [40] ≤2 [50] >2 <4 [>50 <100] ≥4 [100] — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn C-Mn C-Mn
Steel and Steel Alloys
87
2 2 2 2 2 2 2 2
CSA CSA CSA CSA CSA MSS MSS MSS
Z245.11 Z245.11 Z245.12 Z245.12 Z245.12 SP75 SP75 SP75
359 386 317 359 386 WPHY-56 WPHY-60 WPHY-65
— — — — — — — —
— — — — — — — —
66/52 [455/359] 71/56 [490/386] 63/46 [434/317] 66/52 [455/359] 71/56 [490/386] 71/56 [490/386] 75/60 [517/414] 77/65 [531/448]
Steel Fittings Steel Fittings Steel Flanges Steel Flanges Steel Flanges Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 333 A 350 A 350 A 537 A 537 A 537 A 537 A 537 A 537 A 572 A 572 A 607 A 607 A 607 A 611 A 633 A 633 A 656 A 663
Grade 10 Grade LF6, Class 2 Grade LF6, Class 3 Class 2 Class 2 Class 2 Class 3 Class 3 Class 3 Grade 60 Grade 65 Grade 60 Grade 65 Grade 70 Grade E Grade E Grade E Grade 80 Grade 70
— K12202 K12202 K02400 K02400 K02400 K02400 K02400 K02400 K02305 K02306 — — — G10170 K12202 K12202 K11804 —
— — — ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] >4.0 ≤6.0 [>100 ≤150] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] >4.0 ≤6.0 [>100 ≤150] — — — — — — ≤4.0 [100] >4.0 ≤6.0 [>100 ≤150] ≤0.75 [19] —
80/65 [552/448] 75/60 [517/414] 75/60 [517/414] 80/60 [552/414] 75/55 [517/379] 70/46 [483/317] 80/55 [552/379] 75/50 [517/345] 70/40 [483/276] 75/60 [517/414] 80/65 [552/448] 75/60 [517/414] 80/65 [552/448] 85/70 [586/483] 82/80 [565/552] 80/60 [552/414] 75/55 [517/379] 90/80 [621/552] 70/39 [483/26]
Pipe C-Mn-Si-V-Cb Forging 1.3Mn-Si-V-N Forging 1.3Mn-Si-V-N Plate C-Mn-Si Plate C-Mn-Si Plate C-Mn-Si Plate C-Mn-Si Plate C-Mn-Si Plate C-Mn-Si Plate & Bars C-Mn-Si-Cb-V Shapes C-Mn-Si-Cb-V Sheet & Strip C-Mn-Cb-V Sheet & Strip C-Mn-Cb-V Sheet & Strip C-Mn-Cb-V Sheet & Strip C-Mn HSLA Steel C-Mn-Si-N HSLA Steel C-Mn-Si-N Hi-Str. Lo-Alloy Plate 1.65maxMn-0.6Si-0.18maxC Flat, Round, Square & Hex. C Bar & Shapes
(Continued)
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
88
1
3
ASTM
A 663
Grade 75
—
—
75/41 [517/283]
1
3
ASTM
A 663
Grade 80
—
—
80/44 [552/303]
1 1 1
3 3 3
ASTM ASTM ASTM
A 668 A 668 A 668
Class F Class F Class F
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 671 A 672 A 678 A 678 A 678 A 678 A 691 A 707 A 707 A 707 A 710 A 710 A 710 A 737 A 738 A 738 A 738
Grade CD80 Grade D80 Grade C Grade C Grade C Grade D Grade CMSH-80 Grade L2, Class 3 Grade L3, Class 3 Grade L5, Class 3 Grade A, Class 3 Grade A, Class 3 Grade A, Class 3 Grade C Grade B Grade C Grade C
1 1 1
3 3 3
ASTM ASTM ASTM
A 738 A 765 A 913
Grade C Grade IV Grade 60
≤4.0 [100] >4.0 ≤10.0 [>100 ≤250] >10.0 ≤20.0 [>250 ≤500] K02400 — K02400 — K02204 ≤0.75 [19] K02204 >0.75 ≤1.5 [>19 ≤38] K02204 >1.5 ≤2.0 [>38 ≤50] K12202 ≤3 [75] K02400 — K03301 — K12510 — K20934 — K20747 ≤2.00 [50] K20747 >2.00 ≤4.00 [>50 ≤100] K20747 >4.00 [100] K12202 — K12447 — — ≤2.5 [64] — >2.500 ≤4.00 [>64 ≤100] — >4.0 ≤6.0 [>100 ≤150] K03046 — — — — — —
(Continued)
90/55 [621/379] 85/50 [586/345] 82/48 [565/331]
Flat, Round, Square & Hex. Bar & Shapes Flat, Round, Square & Hex. Bar & Shapes Forging Forging Forging
C
C-Mn C-Mn C-Mn
80/60 [552/414] 80/65 [552/448] 95/75 [655/517] 90/70 [621/483] 85/65 [586/448] 90/75 [621/517] 80/60 [552/414] 75/60 [517/414] 75/60 [517/414] 75/60 [517/414] 85/75 [586/517] 75/65 [517/448] 70/60 [483/414] 80/60 [552/414] 85/60 [586/414] 80/60 [552/414] 75/55 [517/379]
Fusion Welded Pipe Fusion Welded Pipe Structural-Plate Structural-Plate Structural-Plate Structural-Plate Fusion Welded Pipe Forging Forging Forging Plate Plate Plate Plate Plate Plate Plate
C-Mn-Si C-Mn-Si 1.3Mn-0.35Si 1.3Mn-0.35Si 1.3Mn-0.35Si 1.33Mn-0.33Si-0.75V-0.20N C-Mn-Si C-1Mn 1.3Mn-V-N 1.2Cu-0.9Ni-0.7Cr-0.5Mn Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb C-Mn-Si-V C-Mn-Si C-Mn-Si C-Mn-Si
70/46 [483/317] 80/50 [552/345] 75/60 [517/414]
Plate Forging Structural Shapes
C-Mn-Si C-Mn-Si C-Mn
C
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
89
3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ABS
A 913 A 935 A 935 A 935 A 935 A 1008 A 1008 A 1011 A 1011 A 1011 ABS
Grade 65 — Grade 65, Class 1 — Grade 65, Class 2 — Grade 70, Class 1 — Grade 70, Class 2 — SS Grade 80 — HSLAS Grade 70 cl 2 — HSLAS Grade 60 cl 1 — HSLAS Grade 65 cl 1 — HSLAS Grade 65 cl 2 — Grade AH40 K11857
— — — — — — — — — — —
80/65 [552/448] 80/65 [552/448] 75/65 [517/448] 85/70 [586/483] 80/70 [552/483] 82/80 [565/552] 80/70 [552/483] 75/60 [517/414] 80/65 [552/448] 75/65 [517/448] 74/57 [510/393]
1
3
ABS
ABS
Grade DH40
K11857
—
74/57 [510/393]
1
3
ABS
ABS
Grade EH40
K11857
—
74/57 [510/393]
1
3
ABS
ABS
Grade FH40
K11857
—
74/57 [510/393]
1 1 1 1 1 1 1 1 1 1 1
3 3 3 3 3 3 3 3 3 3 3
API API AS/NZS CSA CSA CSA CSA CSA CSA CSA CSA
5L 5L 1594 G40.20/40.21 G40.20/40.21 G40.20/40.21 G40.20/40.21 Z245.1 Z245.1 Z245.1 Z245.11
Grade X65 Grade X70 XF500 480A 480AT 480W 480WT 414 448 483 414
— — — — — — — — — — —
— — — — — — — — — — —
77/65 [531/448] 82/70 [565/483] 83/70 [572/483] 85/70 [586/483] 85/70 [586/483] 85/70 [586/483] 85/70 [586/483] 75/60 [517/414] 77/65 [531/448] 82/70 [565/483] 75/60 [517/414]
(Continued)
Structural Shapes Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Sheet Sheet Sheet & Strip Sheet & Strip Sheet & Strip Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Ordinary Strength Hull Structural Steel Pipe Pipe Strip HSLA Steel HSLA Steel HSLA Steel HSLA Steel Pipe Pipe Pipe Steel Fittings
C-Mn C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V — — — — — C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Cb-V-Ti C-Mn-Cb-V-Ti C-Mn C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn C-Mn C-Mn C-Mn-Si
AWS B2.1/B2.1M-BMG:2009
1 1 1 1 1 1 1 1 1 1 1
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
90
1 1 1 1 1 1
3 3 3 3 3 3
CSA CSA CSA CSA CSA MSS
Z245.11 Z245.11 Z245.12 Z245.12 Z245.12 SP75
448 483 414 448 483 WPHY-70
— — — — — —
— — — — — —
77/65 [531/448] 82/70 [565/483] 75/60 [517/414] 77/65 [531/448] 82/70 [565/483] 82/70 [565/483]
Steel Fittings Steel Fittings Steel Flanges Steel Flanges Steel Flanges Seamless & Welded Fittings
C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn
1 1 1 1 1 1 1 1 1 1 1 1 1
4 4 4 4 4 4 4 4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM API CSA CSA
A 707 A 724 A 724 A 724 A 913 A 935 A 984 A 1008 A 1011 A 1011 5L Z245.1 Z245.11
Grade L5, Class 4 Grade A Grade B Grade C Grade 70 Grade 70, Class 1 Grade 85 HSLAS Grade 70 cl 1 HSLAS Grade 70 cl 1 HSLAS Grade 70 cl 2 Grade X80 550 550
K20934 K11831 K12031 K12037 — — — — — — — —
— — — — — — — — — — — — —
90/75 [621/517] 90/70 [621/483] 95/75 [655/517] 90/70 [621/483] 90/70 [621/483] 85/70 [586/483] 90/80 [621/552] 85/70 [586/483] 85/70 [586/483] 80/70 [552/483] 90/80 [621/552] 90/80 [621/552] 90/80 [621/552]
Forging Plate Plate Plate Structural Shapes Sheet & Strip Line Pipe Sheet Sheet & Strip Sheet & Strip Pipe Pipe Steel Fittings
1.2Cu-0.9Ni-0.7Cr-0.5Mn C-Mn-Si C-Mn-Si C-Mn-Si 1.6maxMn-0.16maxC C-Mn-Cb-V C
1A 1A 1A 1A 1A 1A 1A
4 4 4 4 4 4 4
ASTM ASTM ASTM CSA CSA CSA CSA
A 615 A 615 A 706 G30.18 G30.18 G30.18 G30.18
Grade 40 Grade 60 — 300R 400R 500R 400W
— — K03011 — — — —
— — — — — — —
60/40 [414/276] 90/60 [621/414] 80/60 [552/414] 60/40 [414/276] 80/50 [552/345] 90/60 [621/414] 80/60 [552/414]
Rebar Rebar Rebar Rebar Rebar Rebar Rebar
C C C C C C C
(Continued)
C-Mn C-Mn C-Mn-Si
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
90/70 [621/483] 55/30 [379/207] 65/37 [448/255] 60/32 [414/221] 53/28 [365/193] 55/30 [379/207] 60/30 [414/207] 65/35 [448/241] 55/30 [379/207] 60/32 [414/221] 60/30 [414/207] 55/30 [379/207] 53/28 [365/193] 55/30 [379/207] 55/30 [379/207] 60/30 [414/207] 65/35 [448/241] 55/30 [379/207] 55/30 [379/207] 55/33 [379/228] 65/35 [448/241] 60/30 [414/207] 60/30 [414/207] 70/60 [483/414] 65/37 [448/255] 55/33 [379/228] 65/37 [448/255] 60/42 [414/290] 70/50 [483/345]
Rebar Tube Plate Seamless Tube Seamless Tube Seamless Tube Seamless Tube Castings Pipe Fittings ERW Tube ERW Tube ERW Tube ERW Tube Seamless Pipe Seamless Pipe Seamless Pipe Castings Pipe Pipe Plate Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Tapered Tube Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Forging Plate
C C-Mo C-0.5Mo C-0.5Mo C-0.5Mo C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo C-0.5Mo C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo C-0.5Mo C-0.5Mo 0.5Cr-0.5Mo 1.5Si-0.5mo C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo C-0.5Mo-Si 0.5Cr-0.5Mo Mn-Ni-Cr-Cu-Cb C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo 2Mn-0.3Mo-Cb LowC-Mn
Steel and Steel Alloys
91
4 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
CSA ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
G30.18 A 161 A 204 A 209 A 209 A 209 A 213 A 217 A 234 A 250 A 250 A 250 A 250 A 335 A 335 A 335 A 352 A 369 A 369 A 387 A 426 A 426 A 426 A 595 A 672 A 691 A 691 A 707 A 945
500W Grade T1 Grade A Grade T1a Grade T1b Grade T1 Grade T2 Grade WC1 Grade WP1 Grade T1a Grade T2 Grade T1 Grade T1b Grade P1 Grade P2 Grade P15 Grade LC1 Grade FP2 Grade FP1 Grade 2, Class 1 Grade CP1 Grade CP15 Grade CP2 Grade C Grade L65 Grade 1/2 CR, Class 1 Grade CM-65 Grade L6, Class 1 Grade 50
— K11522 K11820 K12023 K11422 K11522 K11547 J12524 K12821 K12023 K11547 K11522 K11422 K11522 K11547 K11578 J12522 K11547 K11522 K12143 J12521 J11522 J11547 K11526 K11820 K12143 K11820 K02902 —
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
1A 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
92
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
1 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
AS/NZS ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
3678 A 182 A 182 A 204 A 204 A 302 A 336 A 387 A 672 A 672 A 672 A 691 A 691 A 691 A 871 A 707 A 945
WR350/WR350L0 Grade F1 Grade F2 Grade B Grade C Grade A Grade F1 Grade 2, Class 2 Grade H75 Grade L70 Grade L75 Grade CM-70 Grade CM-75 Grade 1/2 CR, Class 2 Grade 60 Grade L6, Class 2 Grade 65
— K12822 K12122 K12020 K12320 K12021 K12520 K12143 K12021 K12020 K12320 K12020 K12320 K12143 — K02902 —
≤0.75 [19] — — — — — — — — — — — — — — — —
65/49 [448/338] 70/40 [483/276] 70/40 [483/276] 70/40 [483/276] 75/43 [417/296] 75/45 [417/310] 70/40 [483/276] 70/45 [483/310] 75/45 [417/310] 70/40 [483/276] 75/43 [417/296] 70/40 [483/276] 75/43 [417/296] 70/45 [483/310] 75/60 [517/414] 66/52 [455/359] 78/65 [538/448]
Plate Pipe Flanges & Fittings Pipe Flanges & Fittings Plate Plate Plate Forging Plate Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Plate Forging Plate
C-Mn-Cr-Ni-Cu C-0.5Mo 0.5Cr-0.5Mo C-0.5Mo C-0.5Mo Mn-0.5Mo C-0.5Mo 0.5Cr-0.5Mo Mn-0.5Mo C-0.5Mo C-0.5Mo C-0.5Mo C-0.5Mo 0.5Cr-0.5Mo C-Mn-Ni-Cu-Cr-V 2Mn-0.3Mo-Cb LowC-Mn
3 3 3 3 3 3 3 3 3 3
3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 302 A 302 A 302 A 487 A 508 A 508 A 508 A 508 A 508 A 533
Grade B Grade C Grade D Grade 4, Class C Grade 2, Class 1 Grade 2, Class 2 Grade 3, Class 1 Grade 3, Class 2 Grade 4N, Class 3 Type A, Class 1
K12022 K12039 K12054 J13047 K12766 K12766 K12042 K12042 K22375 K12521
— — — — — — — — — —
80/50 [552/345] 80/50 [552/345] 80/50 [552/345] 90/60 [621/414] 80/50 [552/345] 90/65 [621/448] 80/50 [552/345] 90/65 [621/448] 90/70 [621/483] 80/50 [552/345]
Plate & Sheet Plate & Sheet Plate & Sheet Castings Forging Forging Forging Forging Forging Plate
Mn-0.5Mo Mn-0.5Mo-0.5Ni Mn-0.5Mo-0.75Ni 0.5Ni-0.5Cr-0.25Mo-V 0.75Ni-0.5Mo-0.3Cr-V 0.75Ni-0.5Mo-0.3Cr-V 0.75Ni-0.5Mo-Cr-V 0.75Ni-0.5Mo-Cr-V 30.5Ni-2.75Cr-0.5Mo-V Mn-0.5Mo
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
93
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 533 A 533 A 533 A 533 A 533 A 533 A 533 A 541 A 541 A 541 A 541 A 672 A 672 A 672 A 707 A 871
Type A, Class 2 Type B, Class 1 Type B, Class 2 Type C, Class 1 Type C, Class 2 Type D, Class 1 Type D, Class 2 Grade 2, Class 1 Grade 2, Class 2 Grade 3, Class 1 Grade 3, Class 2 Grade J80 Grade J90 Grade H80 Grade L6, Class 3 Grade 65
K12521 K12539 K12539 K12554 K12554 K12529 K12529 K12765 K12765 K12045 K12045 K12554 K12554 K12022 K02902 —
— — — — — — — — — — — — — — — —
90/70 [621/483] 80/50 [552/345] 90/70 [621/483] 80/50 [552/345] 90/70 [621/483] 80/50 [552/345] 90/70 [621/483] 80/50 [552/345] 90/65 [621/448] 80/50 [552/345] 90/65 [621/448] 80/50 [552/345] 90/70 [621/483] 80/50 [552/345] 75/60 [517/414] 80/65 [552/448]
Plate Plate Plate Plate Plate Plate Plate Forging Forging Forging Forging Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Forging Plate
Mn-0.5Mo Mn-0.5Mo-0.5Ni Mn-0.5Mo-0.5Ni Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.25Ni Mn-0.5Mo-0.25Ni 0.75Ni-0.5Mo-0.3Cr-V 0.75Ni-0.5Mo-0.3Cr-V 0.5Ni-0.5Mo-V 0.5Ni-0.5Mo-V Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.75Ni Mn-0.5Mo 2Mn-0.3Mo-Cb C-Mn-Ni-Cu-Cr-V
3
4
ASTM
A 707
Grade L6, Class 4
K02902
—
90/75 [621/517]
Forging
2Mn-0.3Mo-Cb
4 4 4 4 4 4 4 4 4
1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 182 A 199 A 202 A 202 A 213
Grade F11, Class 1 Grade F11, Class 2 Grade F11, Class 3 Grade F12, Class 1 Grade F12, Class 2 Grade T11 Grade A Grade B Grade T11
K11597 K11572 K11572 K11562 K11564 K11597 K11742 K12542 K11597
— — — — — — — — —
60/30 [414/207] 70/40 [483/276] 75/45 [417/310] 60/32 [414/221] 70/40 [483/276] 60/25 [414/172] 75/45 [417/310] 85/47 [586/324] 60/30 [414/207]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Plate Plate Seamless Tube
1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1Cr-0.5Mo 1.25Cr-0.5Mo 0.5Cr-1.25Mn-Si 0.5Cr-1.25Mn-Si 1.25Cr-0.5Mo-Si
(Continued)
AWS B2.1/B2.1M-BMG:2009
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
60/32 [414/221] 70/40 [483/276] 70/40 [483/276] 70/40 [483/276] 60/30 [414/207] 60/32 [414/221] 60/30 [414/207] 60/30 [414/207] 60/32 [414/221] 60/30 [414/207] 70/40 [483/276] 75/45 [417/310] 70/40 [483/276] 60/30 [414/207] 60/32 [414/221] 60/35 [414/241] 75/45 [417/310] 55/33 [379/228] 65/40 [448/276] 70/40 [483/276] 80/50 [552/345] 80/50 [552/345] 70/40 [483/276] 60/30 [414/207] 80/50 [552/345] 55/33 [379/228] 65/40 [448/276] 60/35 [414/241] 75/45 [417/310]
Seamless Tube Castings Castings Castings Pipe Fittings Pipe Fittings ERW Tube Pipe Pipe Forging Forging Forging Forging Forged Pipe Forged Pipe Plate Plate Plate Plate Castings Castings Cast Pipe Cast Pipe Cast Pipe Forging Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe
1Cr-0.5Mo 1Ni-Cr-0.5Mo 0.75Ni-Mo-0.75Cr 1.25Cr-0.5Mo 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1.25Cr-Mo-Si 1Cr-0.5Mo 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1Cr-0.5Mo 1.25Cr-0.5Mo-V 1Cr-1Mo-V 1.25Cr-Mo 1.25Cr-0.5Mo-0.5Mn 1.25Cr-0.5Mo-0.5Mn 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1Cr-0.5Mo
Steel and Steel Alloys
94
4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 213 A 217 A 217 A 217 A 234 A 234 A 250 A 335 A 335 A 336 A 336 A 336 A 336 A 369 A 369 A 387 A 387 A 387 A 387 A 389 A 389 A 405 A 426 A 426 A 541 A 691 A 691 A 691 A 691
Grade T12 Grade WC4 Grade WC5 Grade WC6 Grade WP11, Class 1 Grade WP12, Class 1 Grade T11 Grade P11 Grade P12 Grade F11, Class 1 Grade F11, Class 2 Grade F11, Class 3 Grade F12 Grade FP11 Grade FP12 Grade 11, Class 1 Grade 11, Class 2 Grade 12, Class 1 Grade 12, Class 2 Grade C23 Grade C24 Grade P24 Grade CP11 Grade CP12 Grade 11, Class 4 Grade 1CR, Class 1 Grade 1CR, Class 2 Grade 1.25CR, Class 1 Grade 1.25CR, Class 2
K11562 J12082 J22000 J12072 — K12062 K11597 K11597 K11562 K11597 K11572 K11572 K11564 K11597 K11562 K11789 K11789 K11757 K11757 J12080 J12092 K11591 J12072 J11562 K11572 K11757 K11789 K11757 K11789
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
95
1
ASTM
A 739
Grade B11
K11797
—
70/45 [483/310]
Bar
1.25Cr-0.5Mo
4 4 4 4 4 4
2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM
A 234 A 234 A 234 A 333 A 423 A 423
Grade WP11, Class 2 Grade WP11, Class 3 Grade WP12, Class 2 Grade 4 Grade 1 Grade 2
— — K12062 K11267 K11535 K11540
— — — — — —
70/40 [483/276] 75/45 [417/310] 70/40 [483/276] 60/35 [414/241] 60/37 [414/255] 60/37 [414/255]
Pipe Fittings Pipe Fittings Pipe Fittings Pipe Tube Tube
1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 0.75Cr-0.75Ni-Cu-Al 0.75Cr-0.5Ni-Cu 0.75Ni-0.5Cu-Mo
4
3
ASTM
A 148
Grade 90-60
—
—
90/60 [621/414]
Castings
C
5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 199 A 199 A 199 A 200 A 200 A 200 A 213 A 213 A 217 A 234 A 234 A 250 A 335 A 335 A 336
Grade F21 Grade F22, Class 1 Grade F22, Class 3 Grade T4 Grade T21 Grade T22 Grade T21 Grade T22 Grade T4 Grade T21 Grade T22 Grade WC9 Grade WP22, Class 1 Grade WP22, Class 3 Grade T22 Grade P21 Grade P22 Grade F21 Class 1
K31545 K21590 K21590 K31509 K31545 K21590 K31545 K21590 K31509 K31545 K21590 J21890 K21590 K21590 K21590 K31545 K21590 K31545
75/45 [417/310] 60/30 [414/207] 75/45 [417/310] 60/25 [414/172] 60/25 [414/172] 60/25 [414/172] 60/25 [414/172] 60/25 [414/172] 60/25 [414/172] 60/30 [414/207] 60/30 [414/207] 70/40 [483/276] 60/30 [414/207] 75/45 [417/310] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Seamless Tube Seamless Tube Tube Tube Tube Seamless Tube Seamless Tube Castings Pipe Fittings Pipe Fittings ERW Tube Seamless Pipe Seamless Pipe Forging
3Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-0.5Mo-0.75Si 3Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 2.5Cr-1Mo-0.75Si 3Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo-Mn 2.25Cr-1Mo-Mn 2.25Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo
— — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
4
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/45 [417/310] 60/30 [414/207] 75/45 [417/310] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 75/45 [417/310] 60/30 [414/207] 75/45 [417/310] 60/30 [414/207] 70/40 [483/276] 60/30 [414/207] 75/45 [417/310] 60/30 [414/207] 75/45 [417/310] 75/45 [417/310]
Forging Forging Forging Forged Pipe Forged Pipe Plate Plate Plate Plate Centrifugal Cast Pipe Centrifugal Cast Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded Pipe Bar
3Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo
70/40 [483/276] 90/65 [621/448] 85/55 [586/379] 60/25 [414/172] 60/25 [414/172] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 90/60 [621/414] 90/60 [621/414] 85/60 [586/414]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Castings Castings Castings
5Cr-0.5Mo 5Cr-0.5Mo 9Cr-1Mo 5Cr-0.5Mo 9Cr-1Mo 5Cr-0.5Mo-Si 5Cr-0.5Mo-Ti 5Cr-0.5Mo 9Cr-1Mo 5Cr-0.5Mo 9Cr-1Mo 9Cr-1Mo
Steel and Steel Alloys
96
5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A 5A
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 336 A 336 A 336 A 369 A 369 A 387 A 387 A 387 A 387 A 426 A 426 A 691 A 691 A 691 A 691 A 739
5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B
1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 199 A 199 A 213 A 213 A 213 A 213 A 217 A 217 A 217
Grade F21, Class 3 K31545 Grade F22, Class 1 K21590 Grade F22, Class 3 K21590 Grade FP21 K31545 Grade FP22 K21590 Grade 21, Class 1 K31545 Grade 21, Class 2 K31545 Grade 22, Class 1 K21590 Grade 22, Class 2 K21590 Grade CP21 J31545 Grade CP22 J21890 Grade 3CR, Class 1 K31545 Grade 3CR, Class 2 K31545 Grade 2-1/4CR, Class 1 K21590 Grade 2-1/4CR, Class 2 K21590 Grade B22 K21390 Grade F5 Grade F5a Grade F9 Grade T5 Grade T9 Grade T5b Grade T5c Grade T5 Grade T9 Grade C5 Grade C12 Grade C12A
K41545 K42544 K90941 K41545 K81590 K51545 K41245 K41545 K90941 J42025 J82090 —
— — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
97
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 234 A 234 A 335 A 335 A 335 A 335 A 336 A 336 A 336 A 369 A 369 A 387 A 387 A 426 A 426 A 426 A 691 A 691
Grade WP5 Grade WP9 Grade P5b Grade P5 Grade P5c Grade P9 Grade F5 Grade F5A Grade F9 Grade FP9 Grade FP5 Grade 5, Class 1 Grade 5, Class 2 Grade CP5 Grade CP5b Grade CP9 Grade 5CR, Class 1 Grade 5CR, Class 2
K41545 K90941 K51545 K41545 K41245 K81590 K41545 K42544 K90941 K90941 K41545 K41545 K41545 J42045 J51545 J82090 K41545 K41545
— — — — — — — — — — — — — — — — — —
60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 60/36 [414/248] 80/50 [552/345] 85/55 [586/379] 60/30 [414/207] 60/30 [414/207] 60/30 [414/207] 75/45 [417/310] 90/60 [621/414] 60/30 [414/207] 90/60 [621/414] 60/30 [414/207] 75/45 [417/310]
Pipe Fittings Pipe Fittings Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Forging Forging Forging Forged Pipe Forged Pipe Plate Plate Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Fusion Welded Pipe Fusion Welded Pipe
5Cr-0.5Mo 9Cr-1Mo 5Cr-0.5Mo-Si 5Cr-0.5Mo 5Cr-0.5Mo-Ti 9Cr-1Mo 5Cr-0.5Mo 5Cr-0.5Mo 9Cr-1Mo 9Cr-1Mo 5Cr-0.5Mo 5Cr-0.5Mo 5Cr-0.5Mo 5Cr-0.5Mo 5Cr-1.5Mo 9Cr-1Mo 5Cr-0.5Mo 5Cr-0.5Mo
5B 5B 5B 5B 5B 5B 5B 5B
2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 199 A 213 A 234 A 335 A 336 A 369 A 387
Grade F91 Grade T91 Grade T91 Grade WP91 Grade P91 Grade F91 Grade FP91 Grade 91, Class 2
K90901 K90901 K90901 S50460 S50460 K90901 S50460 S50460
— — — — — — — —
85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414]
Pipe Flanges & Fittings Seamless Tube Seamless Tube Pipe Fittings Seamless Pipe Forging Forged Pipe Plate
9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-1Mo-V
5C
1
ASTM
A 182
Grade F3V
K31830
85/60 [586/414]
Pipe Flanges & Fittings
3Cr-1Mo-0.25V
— (Continued)
AWS B2.1/B2.1M-BMG:2009
5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B 5B
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
98
5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C 5C
1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 336 A 487 A 508 A 541 A 541 A 542 A 542 A 542 A 542 A 542 A 542 A 542 A 832 A 832
Grade F3V Grade 8A Grade 3V Grade 3V Grade 22, Class 3 Type B, Class 4a Type A, Class 4 Type A, Class 4a Type B, Class 4 Type C, Class 4 Type C, Class 4a Type D, Class 4a Grade 21V Grade 22V
K31830 J22091 K31830 K31830 K21390 K21590 K21590 K21590 K21590 K31830 K31830 K31835 K31830 K31835
— — — — — — — — — — — — — —
85/60 [586/414] 85/55 [586/379] 85/60 [586/414] 85/60 [586/414] 85/55 [586/379] 85/60 [586/414] 85/55 [586/379] 85/60 [586/414] 85/55 [586/379] 85/55 [586/379] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414] 85/60 [586/414]
Forging Castings Forging Forging Forging Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate Pressure Vessel Plate
3Cr-1Mo-0.25V 2.25Cr-1Mo 3Cr-1Mo-0.25V 3Cr-1Mo-0.25V 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo-0.25V 3Cr-1Mo-0.25V 2.25Cr-1Mo-V 3Cr-1Mo-0.25V 2.25Cr-1Mo-0.45 Mn-0.3Va-0.13C
5C 5C 5C
3 3 3
ASTM ASTM ASTM
A 542 A 542 A 542
Type A, Class 3 Type B, Class 3 Type C, Class 3
K21590 K21590 K31830
— — —
95/75 [655/517] 95/75 [655/517] 95/75 [655/517]
Plate Plate Plate
2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo-V-Ti-B
5C 5C 5C 5C 5C 5C
4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM
A 487 A 487 A 541 A 542 A 542 A 542
Grade 8, Class B Grade 8, Class C Grade 22, Class 4 Type A, Class 1 Type B, Class 1 Type C, Class1
J22091 J22091 K21390 K21590 K21590 K31830
— — — — — —
105/85 [724/586] 100/75 [689/517] 105/85 [724/586] 105/85 [724/586] 105/85 [724/586] 105/85 [724/586]
Castings Castings Forging Plate Plate Plate
2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo-V-Ti-B
5C 5C
5 5
ASTM ASTM
A 541 A 542
Grade 22, Class 5 Type C, Class 2
K21390 K31830
— —
115/100 [793/689] 115/100 [793/689]
Forging Plate
2.25Cr-1Mo 3Cr-1Mo-0.25V
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
99
5 5
ASTM ASTM
A 542 A 542
Type A, Class 2 Type B, Class 2
K21590 K21590
— —
115/100 [793/689] 115/100 [793/689]
Plate Plate
2.25Cr-1Mo 2.25Cr-1Mo
6 6 6 6 6 6 6 6 6
1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 240 A 268 A 276 A 473 A 473 A 473 A 479 A 479
Grade F6a, Class 1 Type 410 Type 410 Type 410 Type 403 Type 410 Type 414A Type 403 Type 410
S41000 S41000 S41000 S41000 S40300 S41000 S41400 S40300 S41000
— — — — — — — — —
70/40 [483/276] 65/30 [448/207] 60/30 [414/207] 70/40 [483/276] 70/40 [483/276] 70/40 [483/276] 65/35 [448/241] 70/40 [483/276] 70/40 [483/276]
Pipe Flanges & Fittings Plate Tube Bar Forging Forging Forging-Annealed Bars & Shapes-Annealed Bars & Shapes-Annealed
13Cr 13Cr 13Cr 13Cr 12Cr 13Cr 13Cr-2Ni 12Cr 13Cr
6 6 6 6 6 6 6
2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 240 A 268 A 473 A 473 A 473 A 473
F429 Type 429 Type 429 Type 405 Type 420 Type 429 Type 430
S42900 S42900 S42900 S40500 S42000 S42900 S43000
— — — — — — —
60/35 [414/241] 65/30 [448/207] 60/35 [414/241] 60/30 [414/207] 70/35 [483/241] 65/35 [448/241] 70/35 [483/241]
Pipe Flanges & Fittings Plate Tube Forging Forging Forging Forging
15Cr 15Cr 15Cr 13Cr-Al 13Cr 15Cr 17Cr
6 6 6 6 6 6 6 6
3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 217 A 336 A 426 A 479
Grade F6a, Class 2 Grade F6a, Class 3 Grade F6a, Class 4 Grade F6b Grade CA15 Grade F6 Grade CPCA15 Type 414
S41000 S41000 S41000 S41026 J91150 S41000 J91150 S41400
85/55 [586/379] 110/85 [758/586] 130/110 [896/758] 110/90 [758/621] 90/65 [621/448] 85/55 [586/379] 90/65 [621/448] 115/90 [793/621]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Castings Forging Cast Pipe Bars & Shapes
13Cr 13Cr 13Cr 13Cr-0.5Mo 13Cr 13Cr 13Cr 12.5Cr-2Ni-Si
— — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
5C 5C
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
100
6 6 6 6 6 6
3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM
A 487 A 487 A 487 A 487 A 743 A 743
Grade CA15, Class B Grade CA15, Class C Grade CA15, Class D Grade CA15M, Class A CA-15 CA-15M
J91450 J91171 J91171 J91451 J91150 J91151
— — — — — —
90/65 [621/448] 90/60 [621/414] 100/75 [689/517] 90/65 [621/448] 90/65 [621/448] 90/65 [621/448]
Castings Castings Castings Castings Castings Castings
13Cr 13Cr 13Cr 13Cr 12.7Cr 12.7Cr-0.58Mo
6 6 6 6 6 6 6 6 6 6 6 6
4 4 4 4 4 4 4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 240 A 268 A 352 A 479 A 487 A 487 A 731 A 743 A 743 A 743 A 815
Grade F6NM S41500 S41500 Grade CA6NM S41500 Grade CA6NM, Class A Grade CA6NM, Class B S41500 CA-40 CB-6 CA-6NM S41500
S41500 S41500 S41500 J91540 S41500 J91540 J91540 S41500 J91153 J91804 J91540 S41500
— — — — — — — — — — — —
115/90 [793/621] 115/90 [793/621] 115/90 [793/621] 110/80 [758/552] 115/90 [793/621] 110/80 [758/552] 100/75 [689/517] 115/90 [793/621] 100/70 [689/483] 115/85 [793/586] 110/80 [758/552] 110/90 [758/621]
Pipe Flanges & Fittings Plate Seamless & Welded Tube Castings Bars & Shapes Castings Castings Seamless & Welded Pipe Castings Castings Castings Pipe Fittings
13Cr-4.5Ni-Mo 13Cr-4.5Ni-Mo 13Cr-4.5Ni-Mo 13Cr-4Ni 13Cr-4.5Ni-Mo 13Cr-4Ni 13Cr-4Ni 13Cr-4.5Ni-Mo 12.75Cr 16.5Cr-4.5Ni 12.7Cr-4Ni-0.7Mo 13Cr-4.5Ni-Mo
7 7 7 7 7 7 7 7
1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 240 A 240 A 240 A 268 A 268 A 268 A 268 A 479
Type 405 Type 409 Type 410S S40800 Type 405 Type 409 Type 430 Ti Type 405
S40500 S40900 S41008 S40800 S40500 S40900 S43036 S40500
— — — — — — — —
60/25 [414/172] 55/25 [379/172] 60/30 [414/207] 55/30 [379/207] 60/30 [414/207] 55/30 [379/207] 60/35 [414/241] 60/25 [414/172]
Plate Plate Plate Seamless & Welded Tube Tube Plate Seamless & Welded Tube Bars & Shapes
12Cr-1Al 11Cr-Ti 13Cr 12Cr-Ti 12Cr-1Al 11Cr-Ti 18Cr-Ti-Cb 12Cr-1Al
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
101
2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 240 A 240 A 240 A 240 A 268 A 268 A 268 A 479 A 479 A 479 A 731 A 731 A 803
F430 Type 18-2 Type 430 Type 439 Type XM-27 Type 18Cr-2Mo Type 430 Type 439 S44400 Type 430 Type 439 Type 439 Type 18Cr-2Mo Type 439
S43000 S44400 S43000 S43035 S44627 S44400 S43000 S43035 S44400 S43000 S43035 S43035 S44400 S43035
— — — — — — — — — — — — — —
60/35 [414/241] 60/40 [414/276] 65/30 [448/207] 65/30 [448/207] 65/40 [448/276] 60/40 [414/276] 60/35 [414/241] 60/30 [414/207] 60/45 [414/310] 70/40 [483/276] 70/40 [483/276] 60/30 [414/207] 60/40 [414/276] 60/30 [414/207]
Pipe Flanges & Fittings Plate Plate Plate, Sheet & Strip Plate Seamless & Welded Tube Tube Seamless & Welded Tube Bars & Shapes Bars & Shapes Bars & Shapes Seamless & Welded Pipe Seamless & Welded Pipe Welded Tube
17Cr 18Cr-2Mo 17Cr 17Cr-Ti 27Cr-1Mo 18Cr-2Mo 17Cr 17Cr-Ti 18Cr-2Mo 17Cr 17Cr-Ti 17Cr-Ti 18Cr-2Mo 17Cr-Ti
7
3
ASTM
A 479
Type XM-30
S41040
—
70/40 [483/276]
Bars & Shapes
12.5Cr-Cb
8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182
Grade F304 Grade F304 Grade F304H Grade F304H Grade F304L Grade F304L Grade F304LN Grade F304LN Grade F304N Grade F316 Grade F316 Grade F316H
S30400 S30400 S30409 S30409 S30403 S30403 S30453 S30453 S30451 S31600 S31600 S31609
75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 70/25 [483/172] 65/25 [448/172] 75/30 [517/207] 70/30 [483/207] 80/35 [552/241] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings
18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo
≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] — ≤5.0 [125] >5.0 [125] ≤5.0 [125] (Continued)
AWS B2.1/B2.1M-BMG:2009
7 7 7 7 7 7 7 7 7 7 7 7 7 7
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/30 [483/207] 70/25 [483/172] 65/25 [448/172] 75/30 [517/207] 70/30 [483/207] 80/35 [552/241] 75/30 [517/207] 70/30 [483/207] 70/25 [483/172] 65/25 [448/172] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 75/30 [517/207] 70/30 [483/207] 78/35 [538/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241]
Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube
16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-15Ni-4Si 18Cr-18N-2Si 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N
Steel and Steel Alloys
102
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 182 A 213 A 213 A 213 A 213 A 213 A 213
Grade F316H Grade F316L Grade F316L Grade F316LN Grade F316LN Grade F316N Grade F317 Grade F317 Grade F317L Grade F317L Grade F321 Grade F321 Grade F321H Grade F321H Grade F347 Grade F347 Grade F347H Grade F347H Grade F348 Grade F348 Grade F348H Grade F348H Grade F46 Grade XM-15 TP304 TP304H TP304L TP304LN TP304N
S31609 S31603 S31603 S31653 S31653 S31651 S31700 S31700 S31703 S31703 S32100 S32100 S32109 S32109 S34700 S34700 S34709 S34709 S34800 S34800 S34809 S34809 S30600 S38100 S30400 S30409 S30403 S30453 S30451
>5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] — ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] ≤5.0 [125] >5.0 [125] — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 78/35 [538/241] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 78/30 [538/207] 75/30 [517/207] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 80/35 [552/241]
Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip
16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-15Ni-4Si 16Cr-12Ni-2Mo 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 18Cr-15Ni-4SI 16Cr-12Ni-1Mo 16Cr-12Ni-2Mo-Cb 16Cr-12N-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-Ti 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo-N
Steel and Steel Alloys
103
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240
TP316 TP316H TP316L TP316LN TP316N TP321 TP321H TP347 TP347H TP348 TP348H Type 18-15 Type 316L Type 302 Type 304 Type 304H Type 304L Type 304LN Type 304N Type 305 Type 316 Type 316Cb Type 316H Type 316LN Type 316N Type 316Ti Type 317 Type 317L Type 317LN
S31600 S31609 S31603 S31653 S31651 S32100 S32109 S34700 S34709 S34800 S34809 S30600 S31603 S30200 S30400 S30409 S30403 S30453 S30451 S30500 S31600 S31640 S31609 S31653 S31651 S31635 S31700 S31703 S31753
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 90/50 [621/345] 85/40 [586/276] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207]
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Sheet & Strip Plate Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Seamless & Welded Pipe
18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-18Ni-2Si 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-18Ni-2Si 18Cr-8Ni
Steel and Steel Alloys
104
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 269
Type 321 Type 321H Type 347 Type 347H Type 348 Type 348H Type XM-15 Type XM-21 Type XM-21 TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H TP348 TP348H Type 304 Type 304H Type 304L Type 304LN Type 304N Type 316 Type 316H Type 316L Type XM-15 TP304
S32100 S32109 S34700 S34709 S34800 S34809 S38100 S30452 S30452 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S38100 S30400
— — — — — — — ≤0.1875 [5] >0.1875 [5] — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/25 [483/172] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/25 [517/172] 75/30 [517/207] 75/30 [517/207] 75/25 [517/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207]
Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Bar Bar Bar Bar Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe
18Cr-8Ni 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-8Ni-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo
Steel and Steel Alloys
105
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 269 A 270 A 271 A 271 A 271 A 271 A 271 A 271 A 271 A 271 A 276 A 276 A 276 A 276 A 312 A 312 A 312 A 312 A 312 A 312 A 312
TP304L TP316 TP316L Type 304LN Type 316LN Type 317 Type 321 Type 347 Type 348 Type 304 Type 304 Type 304H Type 316 Type 316H Type 321 Type 321H Type 347 Type 347H Type 304 Type 304L Type 316 Type 316L TP304 TP304H TP304L TP304LN TP304N TP316 TP316H
S30403 S31600 S31603 S30453 S31653 S31700 S32100 S34700 S34800 S30400 S30400 S30409 S31600 S31609 S32100 S32109 S34700 S34709 S30400 S30403 S31600 S31603 S30400 S30409 S30403 S30453 S30451 S31600 S31609
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 70/30 [483/207] 65/25 [448/172] 70/30 [483/207] 80/35 [552/241] 70/30 [483/207] 70/30 [483/207] 65/25 [448/172] 70/30 [483/207] 80/35 [552/241] 70/x30 [483/207] 70/30 [483/207] 70/30 [483/207]
Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless Pipe Seamless Pipe Welded Pipe Seamless Pipe Seamless Pipe Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging
16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-18Ni-2Si 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb
Steel and Steel Alloys
106
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336 A 336
TP316L TP316LN TP316N TP317 TP317L TP321 TP321 TP321 TP321H TP321H TP321H TP347 TP347H TP348 TP348H TPXM-15 F304 F304H F304L F304LN F304N F316 F316H F316L F316LN F316N F321 F321H F347
S31603 S31653 S31651 S31700 S31703 S32100 S32100 S32100 S32109 S32109 S32109 S34700 S34709 S34800 S34809 S38100 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S32109 S34700
— — — — — ≤3/8 [10] >3/8 [10] — ≤3/8 [10] >3/8 [10] — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/30 [483/207] 70/30 [483/207] 65/25 [448/172] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 77/35 [531/241] 70/30 [483/207] 70/30 [483/207] 77/35 [531/241] 70/30 [483/207] 70/30 [483/207] 75/35 [517/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/35 [517/241] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207]
Forging Forging Forging Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Castings Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Seamless Pipe Seamless Pipe
18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 19Cr-9Ni-5Mo 19Cr-9Ni-5Mo 16Cr-14Ni-2Mo 18Cr-8Ni 18Cr-8Ni 18Cr-12Ni-2Mo 18Cr-8Ni 18Cr-8Ni 18Cr-10Ni-Cb 18Cr-12Ni-2Mo 19Cr-10Ni-3Mo 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 16Cr-8Ni-2Mo 18Cr-8Ni
Steel and Steel Alloys
107
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 336 A 336 A 336 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 351 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 358 A 376 A 376
F347H F348 F348H CF10 CF10M CF10MC CF3 CF3A CF3M CF8 CF8A CF8C CF8M CG8M 304 304H 304L 304LN 304N 316 316H 316L 316LN 316N 321 347 348 16-8-2H TP304
S34709 S34800 S34809 J92590 J92901 J92971 J92700 J92700 J92800 J92600 J92600 J92710 J92900 J93000 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S34700 S34800 S16800 S30400
— — — — — — — — — — — — — — — — — — — — — — — — — — — — ≤Schedule 140 (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/30 [483/207] 75/30 [517/207] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207]
Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings
18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti
Steel and Steel Alloys
108
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 376 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403 A 403
TP304 TP304H TP304LN TP304N TP316 TP316H TP316LN TP316N TP321 TP321 TP321H TP321H TP347 TP347H TP348 WP304 WP304H WP304L WP304LN WP304N WP316 WP316H WP316L WP316LN WP316N WP317 WP317L WP321 WP321H
S30400 S30409 S30453 S30451 S31600 S31609 S31653 S31651 S32100 S32100 S32109 S32109 S34700 S34709 S34800 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32109
>Schedule 140 — — — — — — — ≤3/8 [10] >3/8 [10] ≤3/8 [10] >3/8 [10] — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 75/35 [517/241] 70/30 [483/207] 70/30 [483/207] 75/35 [517/241] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 77/35 [531/241] 70/30 [483/207] 70/30 [483/207] 77/35 [531/241]
Pipe Fittings Pipe Fittings Pipe Fittings Pipe Fittings Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Forged Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe
18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 16Cr-8Ni-2Mo 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 16Cr-14Ni-2Mo 18Cr-8Ni 18Cr-8Ni 16Cr-12Ni-2Mo 18Cr-8Ni 18Cr-8Ni
Steel and Steel Alloys
109
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 403 A 403 A 403 A 403 A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 409 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 430 A 451 A 451 A 451 A 451 A 451 A 451
WP347 WP347H WP348 WP348H TP304 TP304L TP316 TP316L TP317 TP321 TP347 TP348 FP16-8-2H FP304 FP304H FP304N FP316 FP316H FP316N FP321 FP321H FP347 FP347H CPF10MC CPF3 CPF3A CPF3M CPF8 CPF8A
S34700 S34709 S34800 S34809 S30400 S30403 S31600 S31603 S31700 S32100 S34700 S34800 S16800 S30400 S30409 S30451 S31600 S31609 S31651 S32100 S32109 S34700 S34709 J92971 J92500 J92500 J92800 J92600 J92600
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/30 [483/207] 70/30 [483/207] 75/30 [517/207] 75/30 [517/207] 75/90 [517/621] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 65/25 [448/172] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 65/25 [448/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207]
Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Centrifugal Cast Pipe Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Bar Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes
18Cr-10Ni-Cb 18Cr-12Ni-2Mo 18Cr-8Ni 16Cr-12Ni-2Mo 18Cr-10Ni-Cb 18Cr-5Ni-9Mn 18Cr-8Ni-Si 18Cr-8Ni-S 18Cr-8Ni-Se 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-12Ni 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo-Cb 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N
Steel and Steel Alloys
110
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 451 A 451 A 452 A 452 A 452 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 473 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479
CPF8C CPF8M TP304H TP316H TP347H Type 302 Type 302B Type 303 Type 303Se Type 304 Type 304 Type 304L Type 305 Type 316 Type 316 Type 316L Type 317 Type 321 Type 347 Type 348 304H 304H 304L 304LN 304N 316Cb 316H 316L 316LN
J92710 J92900 S30409 S31609 S34709 S30200 S30215 S30300 S30323 S30400 S30400 S30403 S30500 S31600 S31600 S31603 S31700 S32100 S34700 S34800 S30409 S30409 S30403 S30453 S30451 S31640 S31609 S31603 S31653
— — — — — — — — — ≤5 [125] >5 [125] — — ≤5 [125] >5 [125] — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 78/35 [538/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 70/25 [483/172] 80/35 [552/241] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 70/30 [483/207]
Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Castings
16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 17Cr-14Ni-4Si 18Cr-8Ni 18Cr-8Ni 16Cr-12Ni-2Mo 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 17Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 19Cr-10Ni
Steel and Steel Alloys
111
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 479 A 666 A 666 A 666 A 666 A 666 A 666 A 666 A 666 A 688 A 688 A 688 A 688 A 688 A 688 A 688 A 688 A 743
316N 316Ti 321H 347H 348H Type 306 Type 302 Type 304 Type 316 Type 321 Type 347 Type 348 Type 302 Type 304 Type 304L Type 304LN Type 304N Type 316 Type 316L Type 316N TP304 TP304L TP304LN TP304N TP316 TP316L TP316LN TP316N CF-3
S31651 S31635 S32109 S34709 S34809 S30600 S30200 S30400 S31600 S32100 S34700 S34800 S30200 S30400 S30403 S30453 S30451 S31600 S31603 S31651 S30400 S30403 S30453 S30451 S31600 S31603 S31653 S31651 J92500
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
112
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 743 A 774 A 774 A 774 A 774 A 774 A 778 A 778 A 778 A 778 A 778 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813
CF-8 CF-8C CF-8M CF-16F CG-8M CG-12 CF-3M CF-3MN CF -10SMnN CG-3M CN-3M TP304L TP316L TP317L TP321 TP347 TP304L TP316L TP317L TP321 TP347 TPXM-15 TP304 TP304H TP304L TP304LN TP304N TP316 TP316H
J92600 J92710 J92900 J92701 J93000 J93001 J92800 J92804 J92972 J92999 J94652 S30403 S31603 S31703 S32100 S34700 S30403 S31603 S31703 S32100 S34700 S38100 S30400 S30409 S30403 S30453 S30451 S31600 S31609
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 75/35 [517/241] 70/28 [483/193] 70/30 [483/207] 75/37 [517/255] 85/42 [586/290] 75/35 [517/241] 63/25 [434/172] 70/25 [483/172] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 70/25 [483/172] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207]
Castings 19Cr-9.Ni Castings 19.5Cr-10.5Ni Castings 19.5Cr-10.5Ni-2.5Mo Castings 19.5Cr-10.5Ni-0.28Se Castings 19.5Cr-11Ni-3.5Mo Castings 21.5Cr-11.5Ni Castings 19Cr-11Ni-2.5Mo Castings 19.5Cr-11Ni-2.5Mo-0.15N Castings 17Cr-8.5Ni-8Mn-4Si-0.12N Castings 19Cr-11Ni-3.5Mo Castings 25Ni-21Cr-05Mo As Welded Wrought Fittings 18Cr-8Ni As Welded Wrought Fittings 16Cr-12Ni-2Mo As Welded Wrought Fittings 18Cr-13Ni-3Mo As Welded Wrought Fittings 18Cr-10Ni-Ti As Welded Wrought Fittings 18Cr-10Ni-Cb Welded Unannealed Tube 18Cr-8Ni Welded Unannealed Tube 16Cr-12Ni-2Mo Welded Unannealed Tube 18Cr-13Ni-3Mo Welded Unannealed Tube 18Cr-10Ni-Ti Welded Unannealed Tube 18Cr-10Ni-Cb Welded Pipe 18Cr-18Ni-2Si Welded Pipe 18Cr-8Ni Welded Pipe 18Cr-8Ni Welded Pipe 18Cr-8Ni Welded Pipe 18Cr-8Ni-N Welded Pipe 18Cr-8Ni-N Welded Pipe 16Cr-12Ni-2Mo Welded Pipe 16Cr-12Ni-2Mo
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 94/44 [648/303] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 70/25 [483/172] 75/30 [517/207] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207]
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe Cold Worked, Welded Pipe
16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-2Mo 18Cr-13Ni-2Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 20Cr-18Ni-6Mo-Cu-N 18Cr-18Ni-2Si 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb
Steel and Steel Alloys
113
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 813 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814 A 814
TP316L TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H TP348 TP348H S31254 TPXM-15 TP304 TP304H TP304L TP304LN TP304N TP316 TP316H TP316L TP316LN TP316N TP317 TP317L TP321 TP321H TP347 TP347H
S31603 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709 S34800 S34809 S31254 S38100 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S31700 S31703 S32100 S32109 S34700 S34709
— — — — — — — — — — — — — — — — — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 70/30 [483/207] 65/25 [448/172] 70/30 [483/207] 80/35 [552/241] 70/30 [483/207] 70/30 [483/207] 65/25 [448/172] 70/30 [483/207] 80/35 [552/241] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 70/30 [483/207] 65/25 [448/172]
Cold Worked, Welded Pipe Cold Worked, Welded Pipe Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging Forging
18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-10Ni-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb
75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 80/30 [552/207] 75/30 [517/207] 70/30 [483/207] 87/45 [600/310] 87/45 [600/310]
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube
20Cr-10Ni 20Cr-10Ni 20Cr-10Ni 20Cr-10Ni 20Cr-10Ni 20Ni-8Cr 25Cr-20Ni 25Cr-20Ni 21Cr-11Ni-N 21Cr-11Ni-N
Steel and Steel Alloys
114
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 814 A 814 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965 A 965
TP348 TP348H F304 F304H F304L F304LN F304N F316 F316H F316L F316LN F316N F321 F321H F347 F347H F348 F348H
S34800 S34809 S30400 S30409 S30403 S30453 S30451 S31600 S31609 S31603 S31653 S31651 S32100 S32109 S34700 S34709 S34800 S34809
8 8 8 8 8 8 8 8 8 8
2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 167 A 167 A 167 A 167 A 167 A 182 A 182 A 182 A 182 A 213
Type 308 Type 309 Type 309S Type 310 Type 310S F10 F310 F310 F45 TP253MA
S30800 S30900 S30908 S31000 S31008 S33100 S31000 S31000 S30815 S30815
— — — — — — — — — — — — — — — — — — — — — — — — ≤5 [125] >5 [125] — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
84/39 [579/269] 78/37 [538/255] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 87/45 [600/310] 80/35 [552/241] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 87/45 [600/310] 78/37 [538/255] 84/39 [579/269] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207]
Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
25Cr-20Ni-2Mo 25Cr-20Ni-2Mo 23Cr-12Ni-Cb 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni 23Cr-12Ni-Cb 25Cr-20Ni 25Cr-20Ni 25Cr-20Ni-Cb 21Cr-11Ni-N 25Cr-22Ni-2Mo-N 23Cr-12Ni-Cb 23Cr-12Ni-Cb 23Cr-12Ni 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 21Cr-11Ni-N 25Cr-22Ni-2Mo-N 25Cr-22Ni-2Mo-N 23Cr-12Ni-Cb 23Cr-12Ni 23Cr-12Ni-Cb 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni
Steel and Steel Alloys
115
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 213 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249 A 249
TP310MoLN TP310MoLN TP309Cb TP309S TP310Cb TP310S Type 309H Type 309HCb Type 310 Type 310H Type 310HCb S30815 TP310MoLN Type 309HCb Type 309Cb Type 309H Type 309S Type 310Cb Type 310S S30815 Type 310 MoLN Type 310 MoLN TP309Cb TP309H TP309HCb TP309S TP310Cb TP310H TP310S
S31050 S31050 S30940 S30908 S31040 S31008 S30909 S30941 S31000 S31009 S31041 S30815 S31050 S30941 S30940 S30909 S30908 S31040 S31008 S30815 S31050 S31050 S30940 S30909 S30941 S30908 S31040 S31009 S31008
≤0.25 [6] >0.25 [6] — — — — — — — — — <3/16 [5] ≥3/16 [5] — — — — — — — >0.25 [6] ≤0.25 [6] — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 65/40 [448/276] 70/35 [483/241] 75/35 [517/241] 70/35 [483/241] 65/35 [448/241] 87/45 [600/310] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 78/37 [538/255] 84/39 [579/269] 75/30 [517/207] 75/30 [517/207] 80/40 [552/276] 70/30 [483/207] 70/30 [483/207] 65/28 [448/193] 65/28 [448/193] 62/35 [427/241] 75/90 [517/621] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207]
Welded Tube Castings Castings Castings Castings Castings Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Welded Pipe Welded Pipe Seamless & Welded Pipe Forging Castings Castings Castings Castings Castings Castings Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
23Cr-12Ni 58Fe-28Cr-9.5Ni-2Mn-2Si 65Fe-20.5Cr-10Ni-2Mn-2Si 57Fe-26Cr-12.5Ni-2Mn-2Si 51Fe-28Cr-16Ni-2Mn-2Si 49Fe-26Cr-20Ni-2Mn-2Si 21Cr-11Ni-N 23Cr-12Ni-Cb 23Cr-12Ni 23Cr-12Ni-Cb 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni-Cb 25Cr-22Ni-2Mo-N 25Cr-22Ni-2Mo-N 25Cr-20Ni 25Cr-20Ni 25Cr-8Ni-N 25Cr-12Ni 25Cr-12Ni 25Cr-12Ni 25Cr-20Ni 25Cr-20Ni-5Mo 23Cr-12Ni 23Cr-12Ni-Cb 23Cr-12Ni 25Cr-20Ni 25Cr-20Ni-Cb
Steel and Steel Alloys
116
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 249 A 297 A 297 A 297 A 297 A 297 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 312 A 336 A 351 A 351 A 351 A 351 A 351 A 351 A 358 A 358 A 358 A 358 A 358
Type 309 HE HF HH HI HK S30815 TP309Cb TP309H TP309HCb TP309S TP310Cb TP310H TP310HCb TP310MoLN TP310MoLN TP310S F310 CE20N CH10 CH20 CH8 CK20 HK40 309 309Cb 309S 310 310Cb
S30900 J93403 J92603 J93503 J94003 J94224 S30815 S30940 S30909 S30941 S30908 S31040 S31000 S31041 S31050 S31050 S31008 S31000 — J93401 J93402 J93400 J94202 J94204 S30900 S30940 S30908 S31000 S31040
— — — — — — — — — — — — — — ≤0.25 [6] >0.25 [6] — — — — — — — — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
75/30 [517/207] 87/45 [600/310] 75/30 [517/207] 75/30 [517/207] 87/45 [600/310] 75/30 [517/207] 75/30 [517/207] 75/30 [517/207] 70/30 [483/207] 70/30 [483/207] 65/28 [448/193] 70/30 [483/207] 75/30 [517/207]
Welded Pipe Welded Pipe Pipe Fittings Pipe Fittings Welded Pipe Welded Pipe Forging Forging Castings Castings Castings Castings Forging
25Cr-20Ni 21Cr-11Ni-N 23Cr-12Ni 25Cr-20Ni 21Cr-11Ni-N 23Cr-12Ni-Cb 20Cr-10Ni 25Cr-21Ni-Si 24Cr-13.5Ni 19.5Cr-9.5Ni 25Cr-20.5Ni 24Cr-13.5Ni 25Cr-20Ni
90/50 [621/345] 100/55 [689/379] 95/50 [655/345] 90/45 [621/310] 95/50 [655/345] 95/38 [655/262] 90/38 [621/262] 100/60 [689/414] 90/50 [621/345] 100/60 [689/414] 90/50 [621/345] 105/60 [724/414] 100/55 [689/379] 100/60 [689/414] 100/55 [689/379]
Pipe Flanges & Fittings Pipe Flanges & Fittings Seamless Tube Seamless Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Sheet & Strip Plate Sheet & Strip Plate Sheet & Strip Plate Sheet & Strip Plate
21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 17Cr-4Ni-6Mn 18Cr-5Ni-9Mn 18Cr-8Ni-4Si-N 17Cr-4Ni-6Mn 18Cr-5Ni-9Mn 19Cr-6Mn-6Ni-Mo-N 19Cr-6Mn-6Ni-Mo-N 19Cr-6Mn-6Ni-Mo-N 19Cr-6Mn-6Ni-Mo-N 22Cr-13Ni-5Mn 22Cr-13Ni-5Mn 18cr-3Ni-12Mn 18Cr-3Ni-12Mn
Steel and Steel Alloys
117
2 2 2 2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 358 A 358 A 403 A 403 A 409 A 409 A 473 A 473 A 743 A 743 A 743 A 743 A 965
310S 253MA WP309 WP310 253MA TP309Cb Type 308 Type 314 CH-20 CF-20 CK-20 CH-10 F310
S31008 S30815 S30900 S31000 S30815 S30940 S30800 S31400 J93402 J92602 J94202 J93401 S31009
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 213 A 213 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240
FXM-11 FXM-19 TP201 TP202 S21800 Type 201-1 Type 202 Type XM-17 Type XM-17 Type XM-18 Type XM-18 Type XM-19 Type XM-19 Type XM-29 Type XM-29
S21904 S20910 S20100 S20200 S21800 S20100 S20200 S21600 S21600 S21603 S21603 S20910 S20910 S24000 S24000
— — — — — — — — — — — — — — — — — — — — ≤3/16 [5] >3/16 [5] ≤3/16 [5] >3/16 [5] ≤3/16 [5] >3/16 [5] ≤3/16 [5] >3/16 [5] (Continued)
AWS B2.1/B2.1M-BMG:2009
8 8 8 8 8 8 8 8 8 8 8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
95/38 [655/262] 90/38 [621/262] 100/55 [689/379] 100/55 [689/379] 90/50 [621/345] 90/50 [621/345] 90/50 [621/345] 100/55 [689/379] 100/55 [689/379] 100/55 [689/379] 90/50 [621/345] 100/55 [689/379] 90/50 [621/345] 100/55 [689/379] 85/42 [586/290].5 100/55 [689/379] 100/55 [689/379] 100/55 [689/379] 90/45 [621/310] 90/50 [621/345] 90/50 [621/345] 95/50 [655/345] 90/50 [621/345] 90/50 [621/345] 90/50 [621/345] 100/55 [689/379] 100/55 [689/379] 90/50 [621/345] 100/60 [689/414]
Welded Tube Welded Tube Welded Tube Welded Tube Tube Tube Tube Tube Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Forging Forging Castings Welded Pipe Welded Pipe Pipe Fittings Forging Forging Forging Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes Plate Sheet & Strip
17Cr-4Ni-6Mn 18Cr-5Ni-9Mn 22cr-13Ni-5Mn 18Cr-3Ni-12Mn 20Cr-6Ni-9Mn 21Cr-6Ni-9Mn 18Cr-18Ni-9i 22Cr-13Ni-7Mn 18Cr-3Ni-12Mn 18Cr-3Ni-12Mn 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 22Cr-12Ni-5Mn 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 22Cr-13Ni-5Mn 18Cr-5Ni-9Mn 20Cr-6Ni-9Mn 21Cr-6Ni-9Mn 18Cr-8Ni-4Si-N 21Cr-6Ni-9Mn 19Cr-8Mn-6Ni-Mo 19Cr-8Mn-6Ni-Mo 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 21Cr-6Ni-9Mn 21Cr-6Ni-9Mn
Steel and Steel Alloys
118
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 249 A 249 A 249 A 249 A 269 A 269 A 269 A 269 A 269 A 312 A 312 A 312 A 336 A 336 A 351 A 358 A 358 A 403 A 473 A 473 A 473 A 479 A 479 A 479 A 479 A 479 A 479 A 666 A 666
TP201 TP202 TPXM-19 TPXM-29 Type XM-10 Type XM-11 Type XM-15 Type XM-19 Type XM-29 TPXM-29 TP-11 FMX-19 FXM-11 FXM-19 CG6MMN XM-19 XM-29 WPXM-19 Type 202 Type XM-10 Type XM-11 Type 218 XM-11 XM-17 XM-18 XM-19 XM-29 XM-11 XM-11
S20100 S20200 S20910 S24000 S21900 S21904 S38100 S20910 S24000 S24000 S21904 S20910 S21904 S20910 J93790 S22100 S28300 S20910 S20200 S21900 S21904 S21800 S21904 S21600 S21603 S20910 S24000 S21904 S21904
— — — — — — — — — — — — — — — — — — — — — — — — — — — >0.25 [6] ≤0.25 [6] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Plate, Sheet & Strip Welded Tube Castings
Nominal Composition
Steel and Steel Alloys
119
3 3 3
ASTM ASTM ASTM
A 666 A 688 A 743
201 XM-29 CG-6MMN
S20100 S24000 —
— — —
75/38 [517/262] 100/55 [689/379] 85/42 [586/290]
8 8 8 8 8 8 8 8
3 3 3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 813 A 813 A 813 A 814 A 814 A 814 A 965 A 965
TPXM-11 TPXM-19 TPXM-29 TPXM-11 TPXM-19 TPXM-29 FXM-11 FXM-19
S21903 S20910 S24000 S21903 S20910 S24000 S21904 S20910
— — — — — — — —
90/50 [621/345] Welded Pipe 100/55 [689/379] Welded Pipe 100/55 [689/379] Welded Pipe 90/50 [621/345] Cold Worked, Welded Pipe 100/55 [689/379] Cold Worked, Welded Pipe 100/55 [689/379] Cold Worked, Welded Pipe 90/50 [621/345] Forging 100/55 [689/379] Forging
8 8 8 8 8 8 8 8 8 8 8 8 8 8 8 8
4 4 4 4 4 4 4 4 4 4 4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 213 A 213 A 240 A 240 A 240 A 249 A 249 A 249 A 249 A 312 A 312 A 312 A 336 A 358 A 358
F44 317LM 317LMN S31254 317LM 317LMN S31254 S31254 317LM 317LH S31254 317LM 317LM F46 S31254 317LM
S31254 S31725 S31726 S31254 S31725 S31726 S31254 S31254 S31725 S31726 S31254 S31725 S31726 S30600 S31254 S31725
— — — — — — ≤0.187 [5] >0.187 [5] — — — — — — — — (Continued)
94/44 [648/303] 75/30 [517/207] 80/35 [552/241] 94/44 [648/303] 75/30 [517/207] 80/35 [552/241] 98/45 [676/310] 95/45 [655/310] 75/30 [517/207] 80/35 [552/241] 94/44 [648/303] 75/30 [517/207] 80/35 [552/241] 78/32 [538/221] 94/44 [648/303] 75/30 [517/207]
Pipe Flanges & Fittings Seamless Tube Seamless Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Forging Welded Pipe Welded Pipe
17Cr-4Ni-6Mn 18Cr-3Ni-12Mn 22Cr-12.5Ni-Mn2.25Mo-Cb-V-N 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn 20Cr-18Ni-6Mo-Cu 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 20Cr-18Ni-6Mo 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 17Cr-14Ni-4SI 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo
AWS B2.1/B2.1M-BMG:2009
8 8 8
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
120
8 8 8 8 8 8 8 8 8 8 8 8
4 4 4 4 4 4 4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 358 A 376 A 376 A 409 A 409 A 409 A 479 A 479 A 479 A 743 A 813 A 965
317L4 317LM 317L4 S31254 317LM 317L4 S31254 317LM 317L4 CK-3MCuN S31254 F46
S31726 S31725 S31726 S31254 S31725 S31726 S31254 S31725 S31726 J93254 S31254 S30600
— — — — — — — — — — — —
80/35 [552/241] 75/30 [517/207] 80/35 [552/241] 94/44 [648/303] 75/30 [517/207] 80/35 [552/241] 94/44 [648/303] 75/30 [517/207] 80/35 [552/241] 80/38 [552/262] 94/44 [648/303] 78/32 [538/221]
Welded Pipe Seamless Tube Seamless Tube Welded Pipe Welded Pipe Welded Pipe Bars & Shapes Bars & Shapes Bars & Shapes Castings Welded pipe Forging
19Cr-15.5Ni-4Mo 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo 19Cr-15Ni-4Mo 20Cr-18.5Ni-6.5Mo-0.75Cu-N 20Cr-18Ni-6Mo-Cu-N 17Cr-14Ni-4SI
9A 9A 9A 9A 9A 9A 9A 9A 9A 9A 9A 9A 9A 9A
1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 203 A 203 A 234 A 333 A 333 A 334 A 334 A 350 A 350 A 350 A 352 A 420 A 714
Grade FR Grade A Grade B Grade WPR Grade 7 Grade 9 Grade 7 Grade 9 Grade LF9 Grade LF5, Class 1 Grade LF5, Class 2 Grade LC2 Grade WPL9 Grade V, Type E
K22035 K21703 K22103 K22035 K21903 K22035 K21903 K22035 K22036 K13050 K13050 J22500 K22035 K22035
— — — — — — — — — — — — — —
63/46 [434/317] 65/37 [448/255] 70/40 [483/276] 63/46 [434/317] 65/35 [448/241] 63/46 [434/317] 65/35 [448/241] 63/46 [434/317] 63/46 [434/317] 60/30 [414/207] 70/37.5 [483/259] 70/40 [483/276] 63/46 [434/317] 65/46 [448/317]
Pipe Flanges & Fittings Plate Plate Pipe Fittings Pipe Pipe Tube Tube Forging Forging Forging Castings Pipe Fittings Welded Pipe
2Ni-1Cu 2.5Ni 2.5Ni 2Ni-1Cu 2.5Ni 2Ni-1Cu 2.5Ni 2Ni-1Cu 2Ni-1Cu 1.5Ni 1.5Ni 2.5Ni 2Ni-1Cu 2Ni-1Cu
9B
1
ASTM
A 203
Grade D
K31718
65/37 [448/255]
Plate
3.5Ni
— (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
121
1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 203 A 203 A 203 A 333 A 334 A 350 A 352 A 420 A 707 A 707 A 765
Grade E Grade F Grade F Grade 3 Grade 3 Grade LF3, Class 2 Grade LC3 Grade WPL3 Grade L7, Class 1 Grade L7, Class 2 Grade III
K32018 K30018 K32018 K31918 K31918 K32025 J31550 — K32218 K32218 K32026
— ≤2.0 [50] >2.0 [50] — — — — — — — —
70/40 [483/276] 80/55 [552/379] 75/50 [517/345] 65/35 [448/241] 65/35 [448/241] 70/37.5 [483/259] 70/40 [483/276] 65/35 [448/241] 60/42 [414/290] 66/52 [455/359] 70/37.5 [483/259]
Plate Plate Plate Pipe Tube Forging Castings Pipe Fittings Forging Forging Forging
3.5Ni 3.5Ni 3.5Ni 3.5Ni 3.5Ni 3.5Ni 3.5Ni 3.5Ni 3.45Ni 3.45Ni 3.5Ni
9C
1
ASTM
A 352
Grade LC4
J41500
—
70/40 [483/276]
Castings
4.5Ni
10A 10A 10A 10A 10A
1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM
A 225 A 225 A 225 A 487 A 487
Grade C Grade D Grade D Grade 1, Class A Grade 1, Class B
K12524 — 105/70 [724/483] — ≤3.0 [75] 80/60 [552/414] — >3.0 ≤6.0 [>75 ≤150] 75/55 [517/379] J13002 — 85/55 [586/379] J13002 — 90/65 [621/448]
Plate Plate Plate Castings Castings
Mn-0.5Ni-V Mn-0.5Ni-V Mn-0.5Ni-V Mn-V Mn-V
10B
1
ASTM
A 213
Grade T17
60/30 [414/207]
Seamless Tube
1Cr-V
10C 10C 10C 10C
1 1 1 1
ASTM ASTM ASTM ASTM
A 612 A 612 A 841 A 841
— — TMCP, Class 1 TMCP, Class 1
K02900 ≤0.5 [13] K02900 >0.5 [13] — >2.5 ≤4.0 [>64 ≤100] — ≤2.5 [64]
83/50 [572/345] 81/50 [558/345] 65/45 [448/310] 70/50 [483/345]
Plate Plate Plate Plate
C-Mn-Si C-Mn-Si C-Mn-Si+X C-Mn-Si+X
10F 10F
1 1
ASTM ASTM
A 487 A 487
Grade 2, Class A Grade 2, Class B
J13005 J13005
85/53 [586/365] 90/65 [621/448]
Castings Castings
Mn-0.25Mo-V Mn-0.25Mo-V
K12047
—
— — (Continued)
AWS B2.1/B2.1M-BMG:2009
9B 9B 9B 9B 9B 9B 9B 9B 9B 9B 9B
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
122
10F
1
ASTM
A 487
Grade 4, Class C
J13047
—
90/60 [621/414]
Castings
0.5Ni-0.5Cr-0.25Mo-V
10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 182 A 182 A 182 A 182 A 182 A 182 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 240 A 276 A 276 A 276 A 351 A 351 A 351 A 479 A 479 A 479 A 479
F50 F51 F53 F55 F60 F61 Type 255 Type 329 S31200 S31260 S31803 S32205 S32950 — — — — — — — CD4MCu CE8MN CD3MWCuN F255 — — —
S31200 S31803 S32750 S32760 S32205 S32250 S32550 S32900 S31200 S31260 S31803 S32205 S32950 S32101 S32101 S32750 S32760 S32101 S32205 S32550 J93370 J93345 J93380 S32550 S31803 S32101 S32205
— — — — — — — — — — — — — t ≤ 0.187 [5] t > 0.187 [5] — — — — — — — — — — — — (Continued)
100/65 [689/448] 90/65 [621/448] 116/90 [800/621] 109/80 [752/552] 95/70 [655/483] 109/80 [752/552] 110/80 [758/552] 90/70 [621/483] 100/65 [689/448] 100/70 [689/483] 90/65 [621/448] 95/65 [655/448] 100/70 [689/483] 101/77 [696/531] 94/65 [648/448] 116/90 [800/621] 109/80 [752/552] 94/65 [648/448] 95/65 [655/448] 109/80 [752/552] 100/70 [689/483] 95/65 [655/448] 100/70 [689/483] 110/80 [758/552] 90/65 [621/448] 94/65 [648/448] 95/65 [655/448]
Pipe Flanges & Fittings Pipe Flanges & Fittings Flanges & Fittings Flanges & Fittings Flanges & Fittings Flanges & Fittings Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Bars & Shapes Bars & Shapes Bars & Shapes Castings Castings Castings Bars & Shapes Bars & Shapes Bar & Shapes Bar & Shapes
25Cr-6Ni-Mo-N 22Cr-5Ni-3Mo-N 25Cr-7Ni-4Mo-N 25Cr-8Ni-3Mo-W-Cu-N 22.5Cr-5.5Ni -3.25Mo-N 26Cr-5Ni-3.5Mo-2Cu-N 26Cr-5Ni-3.5Mo-2Cu-N 26Cr-4Ni-Mo 25Cr-6Ni-Mo-N 25Cr-6Ni-3Mo 22Cr-5Ni-3Mo-N 22.5Cr-5.5Ni -3.25Mo-N 26Cr-4Ni-Mn-N 21.5Cr-5Mn-1.5Ni-Cu-N 21.5Cr-5Mn-1.5Ni-Cu-N 25Cr-7Ni-4Mo-N 25Cr-8Ni-3Mo-W-Cu-N 21.5Cr-5Mn-1.5Ni-Cu-N 22.5Cr-5.5Ni -3.25Mo-N 26Cr-5Ni-3.5Mo-2Cu-N 26Cr-5Ni-3Mo-2Cu 24Cr-10Ni-3Mo 25Cr-8Ni-3Mo-W-Cu-N 26Cr-5Ni-3Cu-2Mo 22Cr-5Ni-3Mo-N 21.5Cr-5Mn-1.5Ni-Cu-N 22.5Cr-5.5Ni -3.25Mo-N
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
110/80 [758/552] 100/65 [689/448] 101/77 [696/531] 94/65 [648/448] 95/70 [655/483] 110/80 [758/552] 109/80 [752/552] 100/70 [689/483] 87/58 [600/400] 100/65 [689/448] 110/80 [758/552] 116/80 [800/552] 92/64 [634/441] 90/70 [621/483] 90/65 [621/448] 100/65 [689/448] 100/65 [689/448] 100/65 [689/448] 92/64 [634/441] 90/65 [621/448] 87/58 [600/400] 110/80 [758/552] 116/80 [800/552] 90/70 [621/483] 90/70 [621/483] 100/70 [689/483] 101/77 [696/531] 94/65 [648/448] 95/65 [655/448]
Bar & Shapes Seamless & Welded Tube Tubing Tubing Tubing Tubing Tubing Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Tube Seamless & Welded Tube Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe
26Cr-5Ni-3.5Mo-2Cu-N 25Cr-6Ni-Mo-N 21.5Cr-5Mn-1.5Ni-Cu-N 21.5Cr-5Mn-1.5Ni-Cu-N 22.5Cr-5.5Ni -3.25Mo-N 26Cr-5Ni-3.5Mo-2Cu-N 25Cr-8Ni-3Mo-W-Cu-N 26Cr-4Ni-Mo-N 23Cr-4Ni-Mo-Cu-N 23Cr-4Ni-Mo-Cu-N 25Cr-5Ni-3Cu-2Mo 25Cr-7Ni-4Mo-N 18Cr-5Ni-3Mo-N 26Cr-4Ni-Mo 22Cr-5Ni-3Mo-N 25Cr-6Ni-3Mo-N 25Cr-6Ni-Mo-N 25Cr-6Ni-3Mo-N 18Cr-5Ni-3Mo-N 22Cr-5Ni-3Mo-N 29Cr-4Ni-Mo-Cu-N 25Cr-5Ni-3Cu-2Mo 25Cr-7Ni-4Mo-N 26Cr-4Ni-Mo 26Cr-4Ni-Mo 26Cr-4Ni-Mo-N 21.5Cr-5Mn-1.5Ni-Cu-N 21.5Cr-5Mn-1.5Ni-Cu-N 22.5Cr-5.5Ni -3.25Mo-N
Steel and Steel Alloys
123
1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 479 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 789 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790 A 790
— S31200 — — — — — Grade 2950 Grade 2304 Grade 2304 Grade 2550 Grade S32750 S31500 Grade S32900 Grade S31803 S31260 Grade S31200 Grade S31260 Grade S31500 Grade S31803 Grade S32304 Grade S32550 Grade S32750 Grade S32900 Grade S32900 Grade S32950 — — —
S32550 S31200 S32101 S32101 S32205 S32550 S32760 S32950 S32304 S32304 S32550 S32750 S31500 S32900 S31803 S31260 S31200 S31260 S31500 S31803 S32304 S32550 S32750 S32900 S32900 S32950 S32101 S32101 S32205
— — t ≤ 0.187 [5] t > 0.187 [5] — — — — >1.0 [25] O.D. ≤1.0 [25] O.D. — — — — — — — — — — — — — — — — t ≤ 0.187 [5] t > 0.187 [5] — (Continued)
AWS B2.1/B2.1M-BMG:2009
10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
124
10H 10H 10H 10H 10H 10H 10H 10H 10H
1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 790 A 790 A 815 A 815 A 815 A 815 A 890 A 890 A 890
— — S31803 S32205 S32550 S32760 1A 1B 1C
S32550 S32760 S31803 S32205 S32550 S32760 J93370 J93372 J93373
— — — — — — — — —
110/80 [758/552] 109/80 [752/552] 90/65 [621/448] 95/70 [655/483] 110/80 [758/552] 109/80 [752/552] 100/70 [689/483] 100/70 [689/483] 100/65 [689/448]
Seamless & Welded Pipe Seamless & Welded Pipe Wrought Pipe Fittings Wrought Pipe Fittings Welded Pipe Fittings Wrought Pipe Fittings Casting Casting Casting
10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H 10H
1 1 1 1 1 1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 890 A 890 A 890 A 890 A 890 A 928 A 928 A 928 A 995 A 995 A 995 A 995 A 995 A 995
2A 3A 4A 5A 6A 255 2205 — 1B 2A 3A 4A 5A 6A
J93345 J93371 J92205 J93404 J93380 S32550 S32205 S32760 J93372 J93345 J93371 J92205 J93404 J93380
— — — — — — — — — — — — — —
95/65 [655/448] 95/65 [655/448] 90/60 [621/414] 100/75 [689/517] 100/65 [689/448] 110/80 [758/552] 95/65 [655/448] 109/80 [752/552] 100/70 [689/483] 95/65 [655/448] 95/65 [655/448] 90/60 [621/414] 100/75 [689/517] 100/65 [689/448]
Casting Casting Casting Casting Casting Welded Pipe Welded Pipe Welded Pipe Casting Casting Casting Casting Casting Casting
26Cr-5Ni-3.5Mo-2Cu-N 25Cr-8Ni-3Mo-W-Cu-N 22Cr-5Ni-3Mo-N 22.5Cr-5.5Ni -3.25Mo-N 26Cr-5Ni-3.5Mo-2Cu-N 25Cr-8Ni-3Mo-W-Cu-N 25.5Cr-5.25Ni-2Mo-3Cu 25.5Cr-5Ni-2Mo-3Cu-N 25.25Cr-6Ni-3.5M0-1.75CuN 24Cr-10Ni-3.75Mo-N 25.5Cr-5Ni-2Mo-N 22.25-5.5Ni-3Mo-N 25Cr-7Ni-4.5M0-N 25Cr-7.5Ni-3.5Mo-.25N 26Cr-5Ni-3.5Mo-2Cu-N 22.5Cr-5.5Ni -3.25Mo-N 25Cr-8Ni-3Mo-W-Cu-N 25.5Cr-5Ni-2Mo-3Cu-N 24Cr-10Ni-3.75Mo-N 25.5Cr-5Ni-2Mo-N 22.25-5.5Ni-3Mo-N 25Cr-7Ni-4.5M0-N 25Cr-7.5Ni-3.5Mo-.25N
10I 10I 10I 10I
1 1 1 1
ASTM ASTM ASTM ASTM
A 182 A 240 A 240 A 240
Grade FXM-27Cb S44635 Type XM-33 Type XM-27
S44627 S44635 S44626 S44627
— — — —
60/35 [414/241] 90/75 [621/517] 68/45 [469/310] 65/40 [448/276]
Pipe Flanges & Fittings Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip
27Cr-1Mo 25Cr-4Ni-4Mo-Ti 27Cr-1Mo-Ti 27Cr-1Mo
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
125
1 1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 268 A 268 A 268 A 268 A 268 A 336 A 479 A 731 A 731
Type 446-1 Type 446-2 25-4-4 TPXM-33 TPXM-27 Grade FXM-27 Cb Type XM-27 Grade TPXM-27 Grade TPXM-33
S44600 S44600 S44635 S44626 S44627 S44627 S44627 S44627 S44626
— — — — — — — — —
70/40 [483/276] 65/40 [448/276] 90/75 [621/517] 68/45 [469/310] 65/40 [448/276] 60/35 [414/241] 65/40 [448/276] 65/40 [448/276] 65/40 [448/276]
Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Forging Bars & Shapes Seamless & Welded Pipe Seamless & Welded Pipe
27Cr 27Cr 25Cr-4Ni-4Mo-Ti 27Cr-1Mo-Ti 27Cr-1Mo 27Cr-1Mo 27Cr-1Mo 27Cr-1Mo 27Cr-1Mo-Ti
10J 10J 10J 10J 10J
1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM
A 240 A 268 A 268 A 479 A 731
Grade 29-4 Grade 29-4 S44735 Grade 28 S44700
S44700 S44700 S44735 S44700 S44700
— — — — —
80/60 [552/414] 80/60 [552/414] 75/60 [517/414] 70/55 [483/379] 80/60 [552/414]
Plate, Sheet & Strip Seamless & Welded Pipe Seamless & Welded Pipe Bars & Shapes Seamless & Welded Pipe
29Cr-4Mo 29Cr-4Mo 29Cr-4Mo-Ti 29Cr-4Mo 29Cr-4Mo
10K 10K 10K 10K 10K 10K 10K 10K
1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 240 A 240 A 268 A 268 A 479 A 731 A 731 A 803
S44660 Grade S44800 Grade 26-3-3 Grade 29-4-2 Grade 28-4-2 Grade 26-3-3 Grade 29-4-2 Grade 26-3-3
S44660 S44800 S44660 S44800 S44800 S44660 S44800 S44660
— — — — — — — —
85/65 [586/448] 80/60 [552/414] 85/65 [586/448] 80/60 [552/414] 80/60 [552/414] 85/65 [586/448] 70/55 [483/379] 85/65 [586/448]
Plate Plate Seamless & Welded Tube Seamless & Welded Tube Bars & Shapes Seamless & Welded Tube Seamless & Welded Tube Welded Tube
26Cr-3Ni-3Mo 29Cr-4Mo-2Ni 26Cr-3Ni-3Mo 29Cr-4Mo-2Ni 29Cr-4Mo-2Ni 26Cr-3Ni-3Mo 29Cr-4Mo-2Ni 26Cr-3Ni-3Mo
11A 11A 11A 11A
1 1 1 1
ASTM ASTM ASTM ASTM
A 333 A 334 A 353 A 420
Grade 8 Grade 8 — Grade WPL8
K81340 K81340 K81340 K81340
100/75 [689/517] 100/75 [689/517] 100/75 [689/517] 100/75 [689/517]
Seamless & Welded Pipe Tube Plate Pipe
9Ni 9Ni 9Ni 9Ni
— — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
10I 10I 10I 10I 10I 10I 10I 10I 10I
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
126
11A 11A 11A 11A 11A 11A
1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM
A 522 A 522 A 553 A 553 A 707 A 844
Type I Type II Type I Type II Grade L8, Class 1 Grade 9% Ni
K81340 K71340 K81340 K71340 K42247 K81340
— — — — — ≤2 [50]
100/75 [689/517] 100/75 [689/517] 100/85 [689/586] 100/85 [689/586] 60/42 [414/290] 100/85 [689/586]
Forging Forging Plate Plate Forging Pressure Vessel Plate
9Ni 8Ni 9Ni 8Ni 3.35Ni-1.75Cr-0.5Mo-0.3Mn 9Ni-0.29Si
11A 11A 11A
2 2 2
ASTM ASTM ASTM
A 645 A 707 A 734
— Grade L8, Class 2 Type A
K41583 K42247 K21205
— — —
95/65 [655/448] 66/52 [455/359] 77/65 [531/448]
Plate Forging Pressure Vessel Plate
0.5Ni-0.25Mo 3.35Ni-1.75Cr-0.5Mo-0.3Mn C-Mn-1Ni-1Cr-0.3Mo
11A 11A 11A
3 3 3
ASTM ASTM ASTM
A 487 A 487 A 707
Grade 4, Class B Grade 4, Class E Grade L8, Class 3
J13047 J13047 K42247
— — —
105/85 [724/586] 115/95 [793/655] 75/60 [517/414]
Castings Castings Forging
0.5Ni-0.5Cr-0.25Mo-V 0.5Ni-0.5Cr-0.25Mo-V 3.35Ni-1.75Cr-0.5Mo-0.3Mn
11A 11A 11A 11A 11A 11A
4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM
A 533 A 533 A 533 A 533 A 672 A 707
Grade A, Class 3 Grade B, Class 3 Grade C, Class 3 Grade D, Class 3 Grade J100 Grade L8, Class 4
K12521 K12539 K12554 K12529 K12521 K42247
— — — — — —
100/83 [689/572] 100/83 [689/572] 100/83 [689/572] 100/83 [689/572] 100/83 [689/572] 90/75 [621/517]
Plate Plate Plate Plate Fusion Welded Pipe Forging
Mn-0.5Mo Mn-0.5Mo-0.5Ni Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.3Ni Mn-0.5Mo 3.35Ni-1.75Cr-0.5Mo-0.3Mn
11A 11A 11A 11A 11A 11A 11A
5 5 5 5 5 5 5
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 352 A 508 A 508 A 508 A 508 A 543 A 543
Grade LC2-1 Grade 4N, Class 1 Grade 4N, Class 2 Grade 5, Class 1 Grade 5, Class 2 Type B, Class 1 Type B, Class 3
J42215 K22375 K22375 K42365 K42365 K42339 K42339
105/80 [724/552] 105/85 [724/586] 115/100 [793/689] 105/85 [724/586] 115/100 [793/689] 105/85 [724/586] 90/70 [621/483]
Castings Forging Forging Forging Forging Plate Plate
3Ni-10.5Cr-0.5Mo 30.5Ni-1.75Cr-0.5Mo-V 30.5Ni-1.75Cr-0.5Mo-V 30.5Ni-1.75Cr-0.5Mo-V 30.5Ni-1.75Cr-0.5Mo-V 3Ni-1.75Cr-0.5Mo 3Ni-1.75Cr-0.5Mo
— — — — — — — (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
105/85 [724/586] 90/70 [621/483]
Plate Plate
2.75Ni-1.75Cr-0.5Mo 2.75Ni-1.75Cr-0.5Mo
Steel and Steel Alloys
127
5 5
ASTM ASTM
A 543 A 543
Type C, Class 1 Type C, Class 3
K42338 K42338
— —
11B 11B 11B 11B 11B 11B 11B 11B
1 1 1 1 1 1 1 1
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 517 A 592 A 592 A 709 A 709
Grade A Grade A Grade A Grade A Grade A Grade A Grade 100, Type A Grade 100W, Type A
K11856 ≤2.5 [64] K11856 >2.5 ≤6.0 [64 ≤150] K11856 ≤2.5 [64] K11856 >2.5 ≤6.0 [>64 ≤150] K11856 ≤2.5 [64] K11856 >2.5 ≤4.0 [>64 ≤100] K11856 ≤2.5 [64] K11856 ≤2.5 [64]
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 105/90 [724/621] 115/100 [793/689] 105/90 [724/621] 110/100 [758/689] 110/100 [758/689]
Plate Plate Plate Plate Forging Forging Plate & Shapes Plate & Shapes
0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si 0.5Cr-0.25Mo-Si
11B 11B 11B 11B 11B 11B 11B 11B 11B 11B
2 2 2 2 2 2 2 2 2 2
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 517 A 592 A 592 A 709 A 709 A 709 A 709
Grade E Grade E Grade E Grade E Grade E Grade E Grade 100, Type E Grade 100, Type E Grade 100W, Type E Grade 100W, Type E
K21604 K21604 K21604 K21604 K11695 K11695 K21604 K21604 K21604 K21604
≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤3.75 [>64 ≤95] ≤2.5 >2.5 ≤4.0 [>64 ≤100] ≤2.5 >2.5 ≤4.0 [>64 ≤100]
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 105/90 [724/621] 115/100 [793/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621]
Plate Plate Plate Plate Forging Forging Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes
1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu 1.75Cr-0.5Mo-Cu
11B 11B 11B 11B 11B 11B
3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 514 A 514 A 517 A 517
Grade F Grade F Grade H Grade H Grade F Grade H
K11576 K11576 K21604 K21604 K11576 K21604
110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 115/100 [793/689]
Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes Plate Plate
0.75Ni-0.5Cr-0.5Mo-V 0.75Ni-0.5Cr-0.5Mo-V 0.5Ni-0.5Cr-0.25Mo-V 0.5Ni-0.5Cr-0.25Mo-V 0.75Ni-0.5Cr-0.5Mo-V 0.5Ni-0.5Cr-0.25Mo-V
≤2.5 [64] >2.5 ≤6.0 ≤2.5 [64] >2.5 ≤6.0 ≤2.5 [64] ≤2.0 [50] (Continued)
AWS B2.1/B2.1M-BMG:2009
11A 11A
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
128
11B 11B 11B 11B 11B 11B
3 3 3 3 3 3
ASTM ASTM ASTM ASTM ASTM ASTM
A 592 A 592 A 709 A 709 A 709 A 709
Grade F Grade F Grade 100, Type F Grade 100W, Type F Grade 100, Type H Grade 100W, Type H
K11576 ≤2.5 [64] K11576 >2.5 ≤4.0 [>64 ≤100] K11576 ≤2.5 [64] K11576 ≤2.5 [64] K21504 ≤2.5 [64] K21504 ≤2.5 [64]
115/100 [793/689] 105/90 [724/621] 110/100 [758/689] 110/100 [758/689] 110/100 [758/689] 110/100 [758/689]
Forging Forging Plates & Shapes Plate & Shapes Plate & Shapes Plate & Shapes
0.75Ni-0.5Cr-0.5Mo-V 0.75Ni-0.5Cr-0.5Mo-V 0.75Ni-0.5Cr-0.5Mo-V 0.75Ni-0.5Cr-0.5Mo-V 0.5Ni-0.5Cr-0.25Mo-V 0.5Ni-0.5Cr-0.25Mo-V
11B 11B 11B 11B 11B 11B
4 4 4 4 4 4
ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 709 A 709 A 782
Grade B Grade B Grade B Grade 100, Type B Grade 100W Type B Class 1
K11630 ≤2.5 [64] K11630 >2.5 ≤6.0 [>64 ≤150] K11630 ≤1.25 [32] K11630 ≤2.5 [64] K11630 ≤2.5 [64] — —
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 110/100 [758/689] 110/100 [758/689] 97/80 [669/552]
Plate Plate Plate Plate & Shapes Plate & Shapes Pressure Vessel Plate
11B
4
ASTM
A 782
Class 2
—
—
107/90 [738/621]
Pressure Vessel Plate
11B
4
ASTM
A 782
Class 3
—
—
115/100 [793/689]
Pressure Vessel Plate
0.5Cr-0.2Mo-V 0.5Cr-0.2Mo-V 0.5Cr-0.2Mo-V 0.5Cr-0.2Mo-V 0.5Cr-0.2Mo-V 0.96Mn-0.76Cr-0.6 Si-0.4Mo-0.09Zr 0.96Mn-0.76Cr-0.6 Si-0.4Mo-0.09Zr 0.96Mn-0.76Cr-0.6 Si-0.4Mo-0.09Zr
11B 11B 11B 11B 11B 11B 11B 11B 11B 11B
6 6 6 6 6 6 6 6 6 6
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514 A 514
Grade C Grade C Grade J Grade J Grade K Grade K Grade S Grade S Grade T Grade T
K11511 K11511 K11625 K11625 K11523 K11523 — — — —
≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤6.0 [>64 ≤150]
110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621]
Plate Plate Plate Plate Plate Plate Plate Plate Plate Plate
(Continued)
1.2Mn-0.2Mo 1.2Mn-0.2Mo C-0.5Mo C-0.5Mo Mn-Mo-B Mn-Mo-B Mn-Mo-B Mn-Mo-B Mn-Mo-B Mn-Mo-B
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Steel and Steel Alloys
129
6 6 6 6 6 6 6 6
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 517 A 517 A 517 A 517 A 709 A 709 A 709 A 709
Grade J Grade K Grade S Grade T Grade 100, Type C Grade 100W, Type C Grade 100, Type J Grade 100W, Type J
K11625 K11523 — — K11511 K11511 K11625 K11625
≤1.25 [32] ≤2.0 [50] ≤2.0 [50] ≤2.0 [50] ≤2.5 [64] ≤2.5 [64] ≤2.5 [64] ≤2.5 [64]
115/100 [793/689] 115/100 [793/689] 115/100 [793/689] 115/100 [793/689] 110/100 [758/689] 110/100 [758/689] 110/100 [758/689] 110/100 [758/689]
Plate Plate Plate Plate Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes
C-0.5Mo Mn-Mo-B Mn-Mo-B Mn-Mo-B 1.2Mn-0.2Mo 1.2Mn-0.2Mo C-0.5Mo C-0.5Mo
11B 11B 11B 11B 11B 11B 11B 11B
8 8 8 8 8 8 8 8
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 517 A 709 A 709 A 709 A 709
Grade P Grade P Grade P Grade P Grade 100, Type P Grade 100, Type P Grade 100W, Type P Grade 100W, Type P
K21650 K21650 K21650 K21650 K21650 K21650 K21650 K21650
≤2.5 [64] >2.5 ≤6.0 [>64 ≤150] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100] ≤2.5 [64] >2.5 ≤4.0 [>64 ≤100]
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 105/90 [724/621] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621]
Plate Plate Plate Plate Plate & Shapes Plates & Shapes Plate & Shapes Plates & Shapes
1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo 1.25Ni-1Cr-0.5Mo
11B 11B 11B 11B 11B 11B 11B 11B 11B 11B
9 9 9 9 9 9 9 9 9 9
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 517 A 519 A 519 A 709 A 709 A 709 A 709
Grade Q — ≤2.5 [64] Grade Q — >2.5 ≤6.0 [>64 ≤150] Grade Q — ≤2.5 [64] Grade Q — >2.5 ≤6.0 [>64 ≤150] Grade 4130 G41300 — Grade 8630 G86300 — Grade 100, Type Q — ≤2.5 [64] Grade 100, Type Q — >2.5 ≤4 [>64 ≤100] Grade 100W, Type Q — ≤2.5 [64] Grade 100W, Type Q — >2.5 ≤4.0 [>64 ≤100]
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 105/90 [724/621] 75/55 [517/379] 75/55 [517/379] 110/100 [758/689] 100/90 [689/621] 110/100 [758/689] 100/90 [689/621]
Plate Plate Plate Plate Mechanical Tube Mechanical Tube Plate & Shapes Plate & Shapes Plate & Shapes Plate & Shapes
1.3Ni-1.3Cr-0.5Mo-V 1.3Ni-1.3Cr-0.5Mo-V 1.3Ni-1.3Cr-0.5Mo-V 1.3Ni-1.3Cr-0.5Mo-V 1Cr-0.2Mo 0.5Ni-0.5Cr-0.2Mo 1.3Ni-1.3Cr-0.5Mo 1.3Ni-1.3Cr-0.5Mo 1.3Ni-1.3Cr-0.5Mo 1.3Ni-1.3Cr-0.5Mo
(Continued)
AWS B2.1/B2.1M-BMG:2009
11B 11B 11B 11B 11B 11B 11B 11B
Material Group Number Number Standard
Base Metal Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
110/100 [758/689] 100/90 [689/621] 115/100 [793/689] 115/100 [793/689] 115/100 [793/689] 110/100 [758/689] 110/100 [758/689]
Plate & Shapes Plate & Shapes Plate & Shapes Plate Plate Plate & Shapes Plate & Shapes
1.3Ni-0.5Mo 1.3Ni-0.5Mo 1.3Ni-0.5Mo 3Ni-1.75Cr-0.5Mo 2.75Ni-1.75Cr-0.5Mo 1.3Ni-0.5Mo 1.3Ni-0.5Mo
85/70 [586/483] 90/70 [621/483]
Plate & Shapes Plate & Shapes
C-Mn-Ni-Cu-Cr-V C-Mn-Ni-Cu-Cr-V
Plate Plate
C-Mn-Ni-Cu-V C-Mn-Ni-Cu-V
Steel and Steel Alloys K11683 ≤2.5 [64] K11683 >2.5 ≤6.0 [>64 ≤150] K11683 ≤2.0 [50] K42339 — K42338 — K11683 ≤2.5 [64] K11683 ≤2.5 [64]
130
11B 11B 11B 11B 11B 11B 11B
10 10 10 10 10 10 10
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 514 A 514 A 517 A 543 A 543 A 709 A 709
Grade M Grade M Grade M Type B, Class 2 Type C, Class 2 Grade 100, Type M Grade 100W, Type M
11B 11B
11 11
ASTM ASTM
A 709 A 852
Grade HPS70W Grade 70W
— K12043
11B 11B
12 12
ASTM ASTM
A 514 A 514
Grade R Grade R
— —
12A 12A 12A 12A
1 1 1 1
ASTM ASTM ASTM ASTM
A 710 A 710 A 710 A 710
Grade A, Class 2 Grade A, Class 2 Grade A, Class 2 Grade A, Class 2
K20747 ≤2.5 [64] K20747 >2.5 ≤6.0 [>64 ≤150] K20747 <2.00 ≤4.0 <50 ≤100] K20747 >4.0 [100]
72/65 [496/448] 100/90 [689/621] 65/55 [448/379] 60/50 [414/345]
Structural Structural Structural Structural
Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb
12B 12B 12B 12B
1 1 1 1
ASTM ASTM ASTM ASTM
A 710 A 710 A 710 A 710
Grade A, Class 3 Grade A, Class 3 Grade A, Class 3 Grade A, Class 3
K20747 ≤1.25 [32] K20747 >1.25 ≤2.0 [>32 ≤50] K20747 >2.0 ≤4.0 [>50 ≤100] K20747 >4.0 [100]
85/80 [586/552] 85/75 [586/517] 75/65 [517/448] 70/60 [483/414]
Structural Structural Structural Structural
Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb
12C 12C
1 1
ASTM ASTM
A 710 A 710
Grade A, Class 1 Grade A, Class 1
K20747 ≤5/16 [8] K20747 >5/16 ≤3/4 [>8 ≤19]
90/85 [621/586] 90/80 [621/552]
Structural Structural
Ni-Cu-Cr-Mo-Cb Ni-Cu-Cr-Mo-Cb
— —
≤2.5 [64] 110/100 [758/689] >2.5 ≤6.0 [>64 ≤150] 100/90 [689/621]
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Ferrous Alloys
Table D.2 M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
8/2.5 [55/17] 11/3.5 [76/24] 14/5.0 [97/34] 13/4.5 [90/31]
Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet
99.6minAl 99.0minAl 1.2Mn 1.2Mn
14/5.0 [97/34]
Plate & Sheet
1.2Mn
17/6.5 [117/45] 14/5.0 [97/34] 15/5.0 [103/34] 15/5.0 [103/34] 18/6.0 [124/41] 16/– [[110/–] 8.5/2.5 [59/17] 11/3.5 [76/24] 14/5.0 [97/34] 13/4.5 [90/31] 14/5.0 [97/34] 11/3.5 [76/24] 10/3.5 [69/24] 13/4.5 [90/31] 15/5.0 [103/34] 18/6.0 [124/41] 8/2.5 [55/17] 11/3.0 [76/21] 14/5.0 [97/34] 8.5/2.5 [59/17] 11/3.0 [76/21] 14/5.0 [97/34]
Sheet Sheet Plate & Sheet Sheet Plate & Sheet Sheet Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube
1.2Mn-0.4Mg 0.5Mn-0.5Mg 1.5Mg 0.4Mg-0.2Mn Al-1.5Mg 1Mg-0.3Mn 99.6minAl 99.0minAl 1.2Mn 1.2Mn 1.2Mn 0.25Mn 0.25Mn 1.2Mn 1.5Mg Al-1.5Mg 99.6minAl 99.0minAl 1.2Mn 99.6minAl 99.0minAl 1.2Mn
Aluminum and Aluminum Base Alloys
131
ASTM ASTM ASTM ASTM
B 209 B 209 B 209 B 209
1060 1100 3003 Alclad 3003
A91060 A91100 A93003 A83003
21
ASTM
B 209
Alclad 3003
A83003
21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 209 B 209 B 209 B 209 B 209 B 209 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 210 B 211 B 211 B 211 B 221 B 221 B 221
3005 3105 5005 5010 5050 5457 1060 1100 3003 Alclad 3003 3303 3102 Alclad 3102 Alclad 3303 5005 5050 1060 1100 3003 1060 1100 3003
A93005 A93105 A95005 A95010 A95050 A95457 A91060 A91100 A93003 A83003 A93303 A93102 A83102 A83303 A95005 A95050 A91060 A91100 A93003 A91060 A91100 A93003
— — — 0.006–0.499 [0.15–12.5] 0.500–3.000 [13–75] — — — — — — — — — — — — — — — — — — — — — —
(Continued)
AWS B2.1/B2.1M-BMG:2009
21 21 21 21
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
132
21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 221 B 221 B 230 B 234 B 234 B 234 B 236 B 241 B 241 B 241 B 241 B 247 B 247 B 313 B 313 B 313 B 313 B 324 B 345
Alclad 3003 3102 1350 1060 3003 Alclad 3003 1350 1060 1100 3003 Alclad 3003 1100 3003 1100 3003 3005 5050 1350 1060
A83003 A93102 A91350 A91060 A93003 A83003 A91350 A91060 A91100 A93003 A83003 A91100 A93003 A91100 A93003 A93005 A95050 A91350 A91060
— — — — — — — — — — — — — — — — — — —
21
ASTM
B 345
3003
A93003
—
21
ASTM
B 345
Alclad 3003
A83003
—
21 21 21 21 21
ASTM ASTM ASTM ASTM ASTM
B 361 B 361 B 361 B 361 B 396
WP1060 WP1100 WP3003 Alclad 3003 5005
A91060 A91100 A93003 A83003 A95005
— — — — —
13/4.5 [90/31] Ext. Bar, Rod, Wire, Shapes & Tube 11/4.0 [76/28] Ext. Bar, Rod, Wire, Shapes & Tube 8/– [55/–] Wire (Electrical) 8/2.5 [55/17] Drawn Seamless Tube 14/5.0 [97/34] Drawn Seamless Tube 13/4.5 [90/31] Drawn Seamless Tube 8/– [55/–] Bars (Electrical) 8.5/2.5 [59/17] Seamless Pipe & Ext. Tube 11/3.0 [76/21] Seamless Pipe & Ext. Tube 14/5.0 [97/34] Seamless Pipe & Ext. Tube 13/4.5 [90/31] Seamless Pipe & Ext. Tube 11/3.0 [76/21] Die, H& & Rolled Ring Forgings 14/5.0 [97/34] Die, H& & Rolled Ring Forgings 11/3.0 [76/21] Welded Tube 14/5.0 [97/34] Welded Tube 17/6.5 [117/45] Welded Tube 18/6.0 [124/41] Welded Tube 8.5/– [59/–] Rectangular & Square Wire (Electrical) 8.5/2.5 [59/17] Seamless Pipe & Tube (Gas & Oil Trans.) 14/5.0 [97/34] Seamless Pipe & Tube (Gas & Oil Trans.) 13/4.5 [90/31] Seamless Pipe & Tube (Gas & Oil Trans.) 8/– [55/–] Fittings 11/3.5 [76/24] Fittings 14/5.0 [97/34] Fittings 13/4.5 [90/31] Fittings 15/5.0 [103/34] Wire (Electrical) (Continued)
1.2Mn 0.25Mn 99.5minAl 99.6minAl 1.2Mn 1.2Mn 99.5minAl 99.6minAl 99.0minAl 1.2Mn 1.2Mn 99.0minAl 1.2Mn 99.0minAl 1.2Mn 1.2Mn-0.4Mg 1.5Mg 99.5minAl 99.6minAl 1.2Mn 1.2Mn 99.6minAl 99.0Al-Si Al-Mg-1Cu-1.2Mn 1.2Mn 0.8Mg
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
133
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 483 B 483 B 483 B 483 B 483 B 483 B 483 B 491 B 491 B 491 B 491 B 491 B 491 B 547 B 547 B 547 B 547 B 609
1060 1100 1435 3003 3102 5005 5050 1050 1100 1200 1235 3003 3102 1100 3003 Alclad 3003 5050 1350
A91060 A91100 A91435 A93003 A93102 A95005 A95050 A91050 A91100 A91200 A91235 A93003 A93102 A91100 A93003 A83003 A95050 A91350
— — — — — — — — — — — — — — — — — —
8.5/2.5 [59/17] 11/3.5 [76/24] 9.5/3.0 [66/21] 14/5.0 [97/34] 11/3.5 [76/24] 15/5.0 [103/34] 18/6.0 [124/41] 8/2.5 [55/17] 11/3.5 [76/24] 11/3.5 [76/24] 9.5/3.0 [66/21] 14/5.0 [97/34] 11/3.5 [76/24] 11/3.5 [76/24] 14/5.0 [97/34] 13/4.5 [90/31] 18/6.0 [124/41] 8.5/– [59/–]
Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Extruded Tube (Gen. Purpose) Roll Formed & Long. Welded Tube Roll Formed & Long. Welded Tube Roll Formed & Long. Welded Tube Roll Formed & Long. Welded Tube Wire (Electrical)
99.6minAl 99.0minAl 99.35minAl-0.4Fe 1.2Mn 0.25Mn 0.8Mg 1.5Mg 99.5minAl 99.0minAl 99.0minAl 99.35minAl 1.2Mn 0.25Mn 99.0minAl 1.2Mn 1.2Mn 1.5Mg 99.5minAl
22 22
ASTM ASTM
B 209 B 209
3004 Alclad 3004
A93004 A83004
22/8.5 [152/59] 21/8.0 [145/55]
Plate & Sheet Plate & Sheet
1.2Mn-1.0Mg 1.2Mn-1.0Mg
22
ASTM
B 209
Alclad 3004
A83004
22/8.5 [152/59]
Plate & Sheet
1.2Mn-1.0Mg
22 22 22 22 22
ASTM ASTM ASTM ASTM ASTM
B 209 B 209 B 209 B 209 B 209
5052 5154 5252 5254 5454
A95052 A95154 A95252 A95254 A95454
— 0.006–0.499 [0.15–12.5] 0.500–3.000 [13–75] — — — — —
25/9.5 [172/66] 30/11 [207/76] 25/9.5 [172/66] 30/11 [207/76] 31/12 [214/83]
Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet
2.5Mg-0.25Cr 3.5Mg-0.25Cr 2.5Mg-0.25Cr 3.5Mg-0.25Cr 2.75Mg-0.8Mn-0.1Cr
(Continued)
AWS B2.1/B2.1M-BMG:2009
21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21 21
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
134
22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22 22
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 209 B 210 B 210 B 211 B 211 B 221 B 221 B 221 B 221 B 234 B 234 B 241 B 241 B 313 B 313 B 313 B 313 B 361 B 483 B 547 B 547 B 547 B 547 B 547
5652 5052 5154 5052 5154 3004 5052 5154 5454 5052 5454 5052 5454 3004 Alclad 3004 5052 5154 WP5154 5052 3004 Alclad 3004 5052 5154 5454
A95652 A95052 A95154 A95052 A95154 A93004 A95052 A95154 A95454 A95052 A95454 A95052 A95454 A93004 A83004 A95052 A95154 A95154 A95052 A93004 A83004 A95052 A95154 A95454
— — — 0.125 [3] — — — — — — — — — — — — — — — — — — — —
25/9.5 [172/66] 25/9.5 [172/66] 30/11 [207/76] 25/9.5 [172/66] 30/11 [207/76] 23/8.5 [159/59] 25/10 [172/69] 30/11 [207/76] 31/12 [214/83] 25/9.5 [172/66] 31/12 [214/83] 25/10 [172/69] 31/12 [214/83] 22/8.5 [152/59] 21/8.0 [145/55] 25/9.5 [172/66] 30/11 [207/76] 30/– [207/–] 25/9.5 [172/66] 22/8.5 [152/59] 21/8.0 [145/55] 25/9.5 [172/66] 30/11 [207/76] 31/12 [214/83]
Plate & Sheet Drawn Seamless Tube Drawn Seamless Tube Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Drawn Seamless Tubes Drawn Seamless Tubes Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Formed Sheet & Seam Welded Tube Fittings Drawn Tube (Gen. Purpose) Formed Sheet & Arc Welded Tube Formed Sheet & Arc Welded Tube Formed Sheet & Arc Welded Tube Formed Sheet & Arc Welded Tube Formed Sheet & Arc Welded Tube
2.5Mg-0.25Cr-0.01maxMn 2.5Mg-0.25Cr 3.5Mg-0.25Cr 2.5Mg-0.25Cr 3.5Mg-0.25Cr 1.2Mn-1.0Mg 2.5Mg-0.25Cr 3.5Mg-0.25Cr 2.75Mg-0.8Mn-0.1Cr 2.5Mg-0.25Cr 2.75Mg-0.8Mn-0.1Cr 2.5Mg-0.25Cr 2.75Mg-0.8Mn-0.1Cr 1.2Mn-1.0Mg 1.2Mn-1.0Mg 2.5Mg-0.25Cr 3.5Mg-0.25Cr 3.5Mg-0.25Cr 2.5Mg-0.25Cr 1.2Mn-1.0Mg 1.2Mn-1.0Mg 2.5Mg-0.25Cr 3.5Mg-0.25Cr 2.75Mg-0.8Mn-0.1Cr
23
ASTM
B 209
A96061
—
24/– [165/–]
Plate & Sheet
1Mg-0.6Si-0.25Cr
23
ASTM
B 209
6061 (T4, T6, T651) Alclad 6061 (T4, T6, T62, T651)
A86061
0.051–0.499 [1.3–12.5]
23/– [159/–]
Plate & Sheet
1Mg-0.6Si-0.25Cr
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
135
ASTM
B 209
23 23
ASTM ASTM
B 210 B 210
23
ASTM
B 211
23 23 23
ASTM ASTM ASTM
B 221 B 221 B 221
23
ASTM
B 221
23 23
ASTM ASTM
B 221 B 221
23
ASTM
B 221
23 23 23
ASTM ASTM ASTM
B 221 B 234 B 241
23
ASTM
B 241
23
ASTM
B 241
23 23 23
ASTM ASTM ASTM
B 241 B 247 B 247
Alclad 6061 (T4, T6, T62, T651) 6061 (T4, T6) 6063 (T4, T6, T62, T83) 6061 (T4, T6, T62, T651) 6005 (T1, T5) 6005A (T1, T5) 6061 (T1, T4, T5, T6, T651) 6063 (T1, T4, T5, T6) 6105 (T1, T5) 6162 (T5, T55, T6, T65) 6351 (T1, T4, T5, T6) 6463 (T1, T5, T6) 6061 (T4, T6) 6061 (T1, T4, T42, T51, T6, T62) 6063 (T1, T4, T42,T5, T52, T6, T62) 6162 (T5, T55, T6, T65) 6351 (T4, T6) 6061 (T6) 6061 (T6, T652)
A86061
24/– [165/–]
Plate & Sheet
1Mg-0.6Si-0.25Cr
A96061 A96063
0.500–5.000 [13–125] — —
24/– [165/–] 17/– [117/–]
Drawn Seamless Tube Drawn Seamless Tube
1Mg-0.6Si-0.25Cr 0.7Mg-0.4Si
A96061
—
24/– [165/–]
Bar, Rod & Wire
1Mg-0.6Si-0.25Cr
A96005 A96005 A96061
— — —
24/– [165/–] 24/– [165/–] 24/– [165/–]
Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube
0.75Si-0.5Mg 0.7Si-0.55Mg-0.3(Mn-Cr) 1Mg-0.6Si-0.25Cr
A96063
—
17/– [117/–]
Ext. Rod, Bar, Shapes & Tube
0.7Mg-0.4Si
A96105 A96162
— —
24/– [165/–] 24/– [165/–]
Ext. Rod, Bar, Shapes & Tube Ext. Rod, Bar, Shapes & Tube
0.8Si-0.6Mg 0.9Mg-0.6Si
A96351
—
24/– [165/–]
Ext. Rod, Bar, Shapes & Tube
1Si-0.6Mg-0.6Mn
A96463 A96061 A96061
— — —
17/– [117/–] 24/– [165/–] 24/– [165/–]
Ext. Rod, Bar, Shapes & Tube Drawn Seamless Tube Extruded Seamless Pipe & Tube
0.7Mg-0.4Si 1Mg-0.6Si-0.25Cr 1Mg-0.6Si-0.25Cr
A96063
—
17/– [117/–]
Extruded Seamless Pipe & Tube
0.7Mg-0.4Si
A96162
—
24/– [165/–]
Extruded Seamless Pipe & Tube
0.9Mg-0.6Si
A96351 A96061 A96061
— — —
24/– [165/–] 24/– [165/–] 24/– [165/–]
Extruded Seamless Pipe & Tube Die Forgings Rolled Ring Forgings
1Si-0.6Mg-0.6Mn 1Mg-0.6Si-0.25Cr 1Mg-0.6Si-0.25Cr
(Continued)
AWS B2.1/B2.1M-BMG:2009
23
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
136
23 23 23 23 23 23
ASTM ASTM ASTM ASTM ASTM ASTM
B 247 B 247 B 247 B 308 B 313 B 317
23
ASTM
B 345
23
ASTM
B 345
23 23 23 23 23 23 23 23 23
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ISO
B 345 B 429 B 429 B 483 B 483 B 491 B 547 B 632 209
24
ASTM
B 209
24
ASTM
B 209
24
ASTM
B 209
24
ASTM
B 209
6061 (T6, T652) 6151 (T6) 6151 (T6, T652) 6061 (T6) 6061 (T4, T6) 6101 (T6, T61, T64, T65) 6061 (T4, T45, T6, T65) 6063 (T1, T4, T5, T6) 6351 (T4, T6) 6061 (T6) 6063 (T6) 6061 (T4, T6) 6063 (T4, T6) 6063 (T1) 6061 (T4, T6) 6061 (T4, T6) 6082 (T4, T6) 2014 (T3, T4, T45, T6, T65) Alclad 2014 (T3, T4, T45, T6, T65) 2219 (T31, T37, T62, T81, T87) Alclad 2219 (T31, T37, T62, T81, T87)
A96061 A96151 A96151 A96061 A96061 A96101
— — — — — —
24/– [165/–] 24/– [165/–] 24/– [165/–] 24/– [165/–] 24/– [165/–] 11/– [76/–]
H& Forgings Die Forgings Rolled Ring Forgings Standard Structural Shapes Formed Sheet & Seam Welded Tube Ext. Bar, Rod, Wire, Shapes & Tube
1Mg-0.6Si-0.25Cr 0.8Si-0.7Mg-0.25Cr 0.8Si-0.7Mg-0.25Cr 1Mg-0.6Si-0.25Cr 1Mg-0.6Si-0.25Cr 0.55Mg-0.5Si
A96061
—
24/– [165/–]
Extruded Seamless Pipe & Tube
1Mg-0.6Si-0.25Cr
A96063
—
17/– [117/–]
Extruded Seamless Pipe & Tube
0.7Mg-0.4Si
A96351 A96061 A96063 A96061 A96063 A96063 A96061 A96061 A96082
— — — — — — — — —
24/– [165/–] 24/– [165/–] 17/– [117/–] 24/– [165/–] 17/– [117/–] 17/– [117/–] 24/– [165/–] 24/– [165/–] 24/– [165/–]
Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Drawn Tube (Gen. Purpose) Formed & Arc Seam Welded Tube Tread Plate Ext. Rod, Bar, Shapes & Tube
1Si-0.6Mg-0.6Mn 1Mg-0.6Si-0.25Cr 0.7Mg-0.4Si 1Mg-0.6Si-0.25Cr 0.7Mg-0.4Si 0.7Mg-0.4Si 1Mg-0.6Si-0.25Cr 1Mg-0.6Si-0.25Cr 1Si-0.8Mg-0.7Mn
A92014
—
35/– [241/–]
Plate & Sheet
4.45Cu-0.85Si-0.8Mn-0.6Mg
A82014
—
35/– [241/–]
Plate & Sheet
4.45Cu-0.85Si-0.8Mn-0.6Mg
A92219
—
35/– [241/–]
Plate & Sheet
6.3Cu-0.3Mn-0.06Ti-0.17Zr
A82219
—
35/– [241/–]
Plate & Sheet
6.3Cu-0.3Mn-0.06Ti-0.17Zr
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
137
24 24 24 24
ASTM ASTM ASTM ASTM
B 210 B 211 B 211 B 221
— — — —
35/– [241/–] 35/– [241/–] 35/– [241/–] 35/– [241/–]
Drawn Seamless Tube Bar, Rod & Wire Bar, Rod & Wire Ext. Bar, Rod, Wire, Shapes & Tube
4.45Cu-0.85Si-0.8Mn-0.6Mg 4.45Cu-0.85Si-0.8Mn-0.6Mg 6.3Cu-0.3Mn-0.06Ti-0.17Zr 4.45Cu-0.85Si-0.8Mn-0.6Mg
24
ASTM
B 221
A92219
—
35/– [241/–]
Ext. Bar, Rod, Wire, Shapes & Tube
6.3Cu-0.3Mn-0.06Ti-0.17Zr
24
ASTM
B 241
A92014
—
35/– [241/–]
Extruded Seamless Pipe & Tube
4.45Cu-0.85Si-0.8Mn-0.6Mg
24
ASTM
B 241
A92219
—
35/– [241/–]
Extruded Seamless Pipe & Tube
6.3Cu-0.3Mn-0.06Ti-0.17Zr
24 24 24 24
ASTM ASTM ASTM ASTM
A92014 A92014 A92219 A92219
— — — —
35/– [241/–] 35/– [241/–] 35/– [241/–] 35/– [241/–]
Die Forgings H& Forgings Die Forgings H& Forgings
4.45Cu-0.85Si-0.8Mn-0.6Mg 4.45Cu-0.85Si-0.8Mn-0.6Mg 6.3Cu-0.3Mn-0.06Ti-0.17Zr 6.3Cu-0.3Mn-0.06Ti-0.17Zr
25
ASTM
B 209
5083
A95083
40/18 [276/124]
Plate & Sheet
4.5Mg-0.8Mn-0.15Cr
25
ASTM
B 209
5083
A95083
39/17 [269/117]
Plate
4.5Mg-0.8Mn-0.15Cr
25
ASTM
B 209
5083
A95083
38/16 [262/110]
Plate
4.5Mg-0.8Mn-0.15Cr
25
ASTM
B 209
5083
A95083
37/15 [255/103]
Plate
4.5Mg-0.8Mn-0.15Cr
25
ASTM
B 209
5083
A95083
36/14 [248/97]
Plate
4.5Mg-0.8Mn-0.15Cr
25
ASTM
B 209
5086
A95086
35/14 [241/97]
Plate & Sheet
4.0Mg-0.5Mn-0.15Cr
25
ASTM
B 209
5086
A95086
0.051–1.500 [1.25–38] 1.501–3.000 [38–75] 3.001–5.000 [80–125] 5.001–7.000 [125–175] 7.001–8.000 [175–200] 0.020–2.000 [0.50–50] 2.001–3.000 [50–76]
34/14 [234/97]
Plate
4.0Mg-0.5Mn-0.15Cr
(Continued)
AWS B2.1/B2.1M-BMG:2009
A92014 A92014 A92219 A92014
B 247 B 247 B 247 B 247
2014 (T4, T6) 2014 (T4, T6) 2219 (T851) 2014 (T4, T45, T6, T65) 2219 (T31, T35, T62, T81, T85) 2014 (T4, T45, T6, T62, T65) 2219 (T31, T35, T62, T81, T85) 2014 (T4, T6) 2014 (T6, T652) 2219 (T6) 2219 (T6, T852)
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
42/19 [290/131]
Plate & Sheet
5.1Mg-0.8Mn-0.1Cr
41/18 [283/124]
Plate
5.1Mg-0.8Mn-0.1Cr
40/17 [276/117]
Plate
5.1Mg-0.8Mn-0.1Cr
39/16 [269/110]
Plate
5.1Mg-0.8Mn-0.1Cr
Aluminum and Aluminum Base Alloys
138
25
ASTM
B 209
5456
A95456
38/15 [262/103]
Plate
5.1Mg-0.8Mn-0.1Cr
A95083 A95086 A95456 A95056 A85056 A95083 A95086 A95456 A95083 A95086 A95456 A95083 A95083 A95086 A95083 A95086 A95083 A95086
0.051–1.500 [1.25–38] 1.501–3.000 [38–76] 3.001–5.000 [80–125] 5.001–7.000 [125–175] 7.001–8.000 [175–200] — — — — — — — — — — — — — — — — — —
25
ASTM
B 209
5456
A95456
25
ASTM
B 209
5456
A95456
25
ASTM
B 209
5456
A95456
25
ASTM
B 209
5456
A95456
25 25 25 25 25 25 25 25 25 25 25 25 25 25 25 25 25 25
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 210 B 210 B 210 B 211 B 211 B 221 B 221 B 221 B 241 B 241 B 241 B 247 B 247 B 313 B 345 B 345 B 547 B 547
5083 5086 5456 5056 Alclad 5056 5083 5086 5456 5083 5086 5456 5083 5083 5086 5083 5086 5083 5086
39/16 [269/110] 35/14 [241/97] 41/19 [283/131] 38/– [262/–] 37/– [255/–] 39/16 [269/110] 35/14 [241/97] 41/19 [283/131] 39/16 [269/110] 35/14 [241/97] 41/19 [283/131] 39/16 [269/110] 39/16 [269/110] 35/14 [241/97] 39/16 [269/110] 35/14 [241/97] 40/18 [276/124] 35/14 [241/97]
Drawn Seamless Tube Drawn Seamless Tube Drawn Seamless Tube Bar, Rod & Wire (Cold Finished) Bar, Rod & Wire (Cold Finished) Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube Ext. Pipe & Tube Ext. Pipe & Tube Ext. Pipe & Tube H& Forgings Die Forgings Formed Sheet & Seam Welded Tube Extruded Seamless Pipe & Tube Extruded Seamless Pipe & Tube Formed & Arc Seam Welded Tube Formed & Arc Seam Welded Tube
4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr 5.1Mg-0.8Mn-0.1Cr 5Mg-0.12Mn-0.12Cu 5Mg-0.12Mn-0.12Cu 4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr 5.1Mg-0.8Mn-0.1Cr 4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr 5.1Mg-0.8Mn-0.1Cr 4.5Mg-0.8Mn-0.15Cr 4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr 4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr 4.5Mg-0.8Mn-0.15Cr 4.0Mg-0.5Mn-0.15Cr
26
ASTM
B 26
208.0 (F)
A02080
—
19/12 [131/83]
Sand Castings
4Cu-3Si
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
139
ASTM ASTM ASTM ASTM ASTM
B 26 B 26 B 26 B 26 B 26
26 26 26 26 26 26 26 26 26 26 26
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 26 B 108 B 108 B 108
26 26
ASTM ASTM
B 108 B 108
26 26 26 26 26 26 26 26
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 108 B 108 B 108 B 108 B 108 B 108 B 618 B 618
222.0 (T61) 319.0 (F, T5, T6) 328.0 (F, T6) 356.0 (F) 356.0 (T51, T6, T7, T71) 443.0 (F) 514.0 (F) 535.0 (F) 705.0 (T5) 710.0 (T5) A356.0 (T6) B443.0 (F) 512.0 (F) 308.0 (F) 319.0 (F, T6) 333.0 (T5, T6, T7) 356.0 (F) 356.0 (T51, T6, T7, T71) 443.0 (F) 513.0 (F) 535.0 (F) A356.0 (T61) A444.0 (T4) B443.0 (F) 208.0 (F) 319.0 (F, T6)
A02220 A03190 A03280 A03560 A03560
— — — — —
23/– [159/–] 23/13 [159/90] 25/14 [172/97] 19/9.5 [131/66] 23/– [159/–]
Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings
10Cu-0.25Mg 6Si-3.5Cu 8Si-1.5Cu-0.4Mg-0.4Mn 7Si-0.35Mg 7Si-0.35Mg
A04430 A05140 A05350 A07050 A07100 A13560 A24430 A05120 A03080 A03190 A03330
— — — — — — — — — — —
17/7 [117/48] 22/9 [152/62] 35/18 [241/124] 30/17 [207/117] 32/20 [221/138] 23/– [159/–] 17/6 [117/41] 17/10 [117/69] 24/– [165/–] 24/14 [165/97] 28/– [193/–]
Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Sand Castings Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting
5.2Si 4Mg 6.8Mg-0.18Mn 3Zn-1.6Mg-0.5Mn-0.3Cr 6.5Zn-0.7Mg-0.47Cu 7Si-0.3Mg 5.2Si 4Mg-1.8Si 5.5Si-4.5Cu 6Si-3.5Cu 9Si-3.5Cu-0.3Mn
A03560 A03560
— —
21/– [145/–] 23/– [159/–]
Permanent Mold Casting Permanent Mold Casting
7Si-0.35Mg 7Si-0.35Mg
A04430 A05130 A05350 A13560 A14440 A24430 A02080 A03190
— — — — — — — —
17/7.0 [117/48] 22/12 [152/83] 35/18 [241/124] 23/– [159/–] 17/– [117/–] 17/6.0 [117/41] 19/12 [131/83] 23/13 [159/90]
Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Investment Castings Investment Castings
5.2Si 4Mg-1.8Zn 6.8Mg-0.18Mn 7Si-0.3Mg 7Si 5.2Si 4Cu-3Si 6Si-3.5Cu
(Continued)
AWS B2.1/B2.1M-BMG:2009
26 26 26 26 26
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Aluminum and Aluminum Base Alloys
140
26 26
ASTM ASTM
B 618 B 618
A03280 A03560
— —
25/14 [172/97] 23/– [159/–]
Investment Castings Investment Castings
8Si-1.5Cu-0.4Mg-0.4Mn 7Si-0.35Mg
B 618 B 618 B 618 B 618 B 618 B 686
328.0 (F, T6) 356.0 (T6, T7, T51, T71) 443.0 (F) 514.0 (F) 535.0 (F) A356.0 (T6) B443.0 (F) A356.0 (T61)
26 26 26 26 26 26
ASTM ASTM ASTM ASTM ASTM ASTM
A04430 A05140 A05350 A13560 A24430 A13560
— — — — — —
17/7.0 [117/48] 22/9.0 [152/62] 35/18 [241/124] 23/– [159/–] 17/6.0 [117/41] 23/– [159/–]
Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings Investment Castings
5.2Si 4Mg 6.8Mg-0.18Mn 7Si-0.3Mg 5.2Si 7Si-0.3Mg
27 27
ASTM ISO
B 221 209
7005 (T53) 7020 (T5)
A97005 A97020
— —
40/– [276/–] 40/– [276/–]
Ext. Bar, Rod, Wire, Shapes & Tube Ext. Bar, Rod, Wire, Shapes & Tube
4.5Zn-1.4Mg-0.45Mn-0.13Cr 4.5Zn-1.2Mg-0.25Mn-0.18Cr
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
141
ASTM
B 42
31
ASTM
B 42
31
ASTM
B 42
31
ASTM
B 42
31
ASTM
B 42
31
ASTM
B 68
31
ASTM
B 68
31
ASTM
B 68
31
ASTM
B 68
31
ASTM
B 68
31
ASTM
B 75
31
ASTM
B 75
31
ASTM
B 75
31
ASTM
B 75
31
ASTM
B 75
31
ASTM
B 75
Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu (OFLP) Deoxidized Low P Cu (DLP) Deoxidized High P Cu (DHP) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu (OFLP) Deoxidized Low P Cu (DLP) Deoxidized High P Cu (DHP) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu (OFLP) Deoxidized Low P Cu (DHL) Deoxidized High P Cu (DHP)
C10200
—
30/9 [207/62]
Seamless Pipe
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Pipe
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Pipe
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Pipe
99.90Cu-Ag-0.008P
C12200
—
30/9 [207/62]
Seamless Pipe
99.9Cu-0.027P
C10200
—
30/9 [207/62]
Seamless Tube
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Tube
99.90Cu-Ag-0.008P
C12200
—
30/9 [207/62]
Seamless Tube
99.9Cu-0.027P
C10100
—
30/9 [207/62]
Seamless Tube
99.99Cu-Ag
C10200
—
30/9 [207/62]
Seamless Tube
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Tube
99.9Cu-Ag-0.008P
C12200
—
30/9 [207/62]
Seamless Tube
99.9Cu-0.027P
(Continued)
AWS B2.1/B2.1M-BMG:2009
31
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
142
31
ASTM
B 75
31
ASTM
B 88
31
ASTM
B 88
31
ASTM
B 88
31
ASTM
B 88
31
ASTM
B 111
31
ASTM
B 111
31
ASTM
B 111
31
ASTM
B 111
31
ASTM
B 111
31
ASTM
B 111
31
ASTM
B 111
31 31
ASTM ASTM
B 111 B 152
31
ASTM
B 152
31
ASTM
B 152
Oxygen-Free Cu (DPA) Oxygen Free Cu (OF) Oxygen Free Cu (OFXLP) Oxygen Free Cu (DLP) Oxygen Free Cu (DLP) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (DLP) Oxygen-Free Cu (DHP) Oxygen-Free Cu (DPA) 98.5 min Cu Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP)
C14200
—
30/9 [207/62]
Seamless Tube
99.4Cu-0.3As-0.27P
C10200
—
30/– [207/–]
Seamless Tube
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.003P
C12000
—
30/– [207/–]
Seamless Tube
99.9Cu-0.008P
C12200
—
30/– [207/–]
Seamless Tube
99.9Cu-0.027P
C10100
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.4Cu-0.3Ag-0.27P
C10200
—
36/– [248/–]
Seamless Tube & Ferrule Stock
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.9Cu-Ag
C12200
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.9Cu-0.027P
C14200
—
30/9 [207/62]
Seamless Tube & Ferrule Stock
99.4Cu-0.3Ag-0.27P
C19200 C10100
— —
38/12 [262/83] 30/9 [207/62]
Seamless Tube & Ferrule Stock Plate, Sheet, Strip & Rolled Bar
98.7Cu-1Fe-0.025P 99.4Cu-0.3Ag-0.27P
C10200
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu-Ag
C10300
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu-0.003P
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
143
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 152
31
ASTM
B 170
31
ASTM
B 170
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
Oxygen-Free Cu (OFS) Oxygen-Free Cu (OFS) Oxygen-Free Cu (OFS) Oxygen-Free Cu (OFLP) Oxygen-Free Cu (DLP) Oxygen-Free Cu (DHP) Oxygen-Free Cu (DPS) Oxygen-Free Cu (DPA) Sn Bearing Tellurium Cu Oxygen-Free Electronic Cu (OFE) Oxygen-Free Electronic Cu (OF) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu with Ag (OFS)
C10400
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu0.027Ag
C10500
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu-0.034Ag
C10700
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu-0.085Ag
C10800
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.9Cu-Ag
C12200
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.9Cu-0.027P
C12300
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.9Cu-0.027P
C14200
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.4Cu-0.3Ag-0.27P
C14420
—
30/9 [207/62]
Plate, Sheet, Strip & Rolled Bar
99.9Cu-0.10Sn-0.02Te
C10100
—
30/9 [207/62]
Refinery Shapes
99.4Cu-0.3Ag-0.27P
C10200
—
30/9 [207/62]
Refinery Shapes
99.95Cu-Ag
C10100
—
28/– [193/–]
Rod
99.99Cu
C10200
—
28/– [193/–]
Rod
99.95Cu-Ag
C10300
—
28/– [193/–]
Rod
99.95Cu-0.003P
C10400
—
28/– [193/–]
Rod
99.95Cu-0.027Ag
(Continued)
AWS B2.1/B2.1M-BMG:2009
31
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
144
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
31
ASTM
B 187
Oxygen-Free Cu with Ag (OFS) Controlled Oxygen Cu Sn Bearing Tellurium Cu Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu with Ag (OFS) Oxygen-Free Cu with Ag (OFS) Controlled Oxygen Cu Sn Bearing Tellurium Cu Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Cu with Ag (OFS) Oxygen-Free Cu with Ag (OFS) Controlled Oxygen Cu
C10700
—
28/– [193/–]
Rod
99.95Cu-0.085Ag
C10940
—
28/– [193/–]
Rod
99.90minCu-Ag
C14420
—
28/– [193/–]
Rod
99.9Cu-0.10Sn-0.02Te
C10100
—
28/– [193/–]
Bars
99.99Cu
C10200
—
28/– [193/–]
Bars
99.95Cu-Ag
C10300
—
28/– [193/–]
Bars
99.95Cu-0.003P
C10400
—
28/– [193/–]
Bars
99.95Cu-0.027Ag
C10700
—
28/– [193/–]
Bars
99.95Cu-0.085Ag
C10940
—
28/– [193/–]
Bars
99.90minCu-Bar
C14420
—
28/– [193/–]
Bars
99.9Cu-0.10Sn-0.02Te
C10100
—
28/– [193/–]
Rolled Shapes
99.99Cu
C10200
—
28/– [193/–]
Rolled Shapes
99.95Cu-Ag
C10300
—
28/– [193/–]
Rolled Shapes
99.95Cu-0.003P
C10400
—
28/– [193/–]
Rolled Shapes
99.95Cu0.027Ag
C10700
—
28/– [193/–]
Rolled Shapes
99.95Cu-0.085Ag
C10940
—
28/– [193/–]
Rolled Shapes
99.90minCu-Ag
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
145
ASTM
B 187
31
ASTM
B 280
31
ASTM
B 280
31
ASTM
B 280
31
ASTM
B 359
31
ASTM
B 359
31
ASTM
B 359
31
ASTM
B 359
31
ASTM
B 359
31
ASTM
B 359
31
ASTM
B 359
31 31
ASTM ASTM
B 359 B 395
31
ASTM
B 395
31
ASTM
B 395
31
ASTM
B 395
Sn Bearing Tellurium Cu Oxygen-free Cu (OF) Deoxidized Cu (DLP) Deoxidized Cu (DHP) Oxygen-Free Cu (OFE) Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Low P Cu (OFLP) Deoxidized Low P Cu (DLP) Deoxidized High P Cu (DHP) Deoxidized AsCu (DPA) 98.7 min Cu Oxygen-Free Cu (OF) Oxygen-Free Cu (OFXLP) Oxygen-Free Low P Cu (OFLP) Deoxidized Low P Cu (DLP)
C14420
—
28/– [193/–]
Rolled Shapes
99.9Cu-0.10Sn-0.02Te
C10200
—
—
Seamless Tube
99.95Cu+Ag
C12000
—
—
Seamless Tube
99.9Cu+Ag
C12200
—
30/9 [207/62]
Seamless Tube
99.9Cu-0.027P
C10100
—
30/9 [207/62]
Seamless Tube
99.99Cu
C10200
—
30/9 [207/62]
Seamless Tube
99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Tube
99.9Cu-Ag-0.008P
C12200
—
30/9 [207/62]
Seamless Tube
99.9Cu-0.027P
C14200
—
30/9 [207/62]
Seamless Tube
99.4Cu-0.3As-0.027P
C19200 C10200
— —
30/9 [207/62] 30/9 [207/62]
Seamless Tube Seamless Tube
98.7Cu-1Fe-0.025P 99.95Cu-Ag
C10300
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.003P
C10800
—
30/9 [207/62]
Seamless Tube
99.95Cu-0.008P
C12000
—
30/9 [207/62]
Seamless Tube
99.9Cu-Ag
(Continued)
AWS B2.1/B2.1M-BMG:2009
31
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys ASTM
B 395
31
ASTM
B 395
31 31
ASTM ASTM
B 395 B 543
31
ASTM
B 543
31 31
ASTM ASTM
B 543 B 819
32
ASTM
B 21
32
ASTM
B 21
32
ASTM
B 21
32
ASTM
B 21
32 32 32 32 32 32 32
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 43 B 111 B 111 B 111 B 111 B 111 B 111
32
ASTM
B 135
146
31
Deoxidized High P Cu (DHP) Deoxidized AsCu (DPA) 98.7 min Cu Oxygen-Free Low P Cu (OFLP) Deoxidized High P Cu (DHP) 97.0 min Cu Deoxidized High P Cu (DHP) Alloy A Naval Brass Alloy A Naval Brass Alloy A Naval Brass Alloy A Naval Brass Red Brass, 85% Red Brass, 85% Muntz Metal Admiralty, A Admiralty, B Admiralty, C Aluminum Brass B Commercial Bronze, 90%
C12200
—
30/9 [207/62]
Seamless Tube
99.9Cu-0.027P
C14200
—
30/9 [207/62]
Seamless Tube
99.4Cu-0.3Ag-0.027P
C19200 C10800
— —
30/9 [207/62] 30/9 [207/62]
Seamless Tube Welded Tube
98.7Cu-1Fe-0.025P 99.95Cu-0.008P
C12200
—
30/9 [207/62]
Welded Tube
99.9Cu-0.027P
C19400 C12200
— —
45/15 [310/103] 30/9 [207/62]
Welded Tube Seamless Tube
97Cu-2.3Fe-0.08P 99.9Cu-0.027P
C46400
≤1.00 [25] O.D.
54/20 [372/138]
Rod & Bar
60.5Cu-38Zn-0.75Sn
C46400
52/20 [359/138]
Rod & Bar
60.5Cu-38Zn-0.75Sn
C46400
>1.00 ≤2.00 [>25 ≤50] >2.00 [50]
50/20 [345/138]
Rod & Bar
60.5Cu-38Zn-0.75Sn
C46400
—
52/20 [359/138]
Shapes
60.5Cu-38Zn-0.75Sn
C23000 C23000 C28000 C44300 C44400 C44500 C68700
— — — — — — —
40/12 [276/83] 40/12 [276/83] 50/20 [345/138] 45/15 [310/103] 45/15 [310/103] 45/15 [310/103] 50/18 [345/123]
Seamless Pipe Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock Seamless Tube & Ferrule Stock
85Cu-15Zn 85Cu-15Zn 61Cu-38Zn 71.5Cu-28Zn-1Sn-0.04Ag 71.5Cu-28Zn-1Sn-0.06Sb 71.5Cu-28Zn-1Sn-0.06P 67.5Cu-31Zn-1.9Al-0.04Ag
C22000
—
38/12 [262/83]
Seamless Tube
90Cu-9.8Zn
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
147
ASTM ASTM
B 135 B 171
32
ASTM
B 171
32
ASTM
B 171
32 32 32 32 32 32
ASTM ASTM ASTM ASTM ASTM ASTM
B 171 B 171 B 171 B 171 B 171 B 171
32
ASTM
B 171
32 32 32 32 32
ASTM ASTM ASTM ASTM ASTM
B 359 B 359 B 359 B 359 B 359
32 32 32 32 32
ASTM ASTM ASTM ASTM ASTM
B 395 B 395 B 395 B 395 B 395
32 32
ASTM ASTM
B 543 B 543
Red Brass, 85% Leaded Muntz Metal Leaded Muntz Metal Leaded Muntz Metal Admiralty, A Admiralty, B Admiralty, C Naval Brass Naval Brass Naval Brass, Arsenical Naval Brass, Arsenical Red Brass, 85% Admiralty, A Admiralty, B Admiralty, C Aluminum Brass B Red Brass, 85% Admiralty, A Admiralty, B Admiralty, C Aluminum Brass B Red Brass, 85% Admiralty, A
C23000 C36500
— ≤2.00 [50]
40/12 [276/83] 50/20 [345/138]
Seamless Tube Plate & Sheet
85Cu-15Zn 59.5Cu-40Zn-0.5Pb
C36500
45/15 [310/103]
Plate & Sheet
59.5Cu-40Zn-0.5Pb
40/12 [276/83]
Plate & Sheet
59.5Cu-40Zn-0.5Pb
C44300 C44400 C44500 C46400 C46400 C46500
>2.0 ≤3.5 [>50 ≤89] >3.5 ≤5.0 [>89 ≤125] ≤4.0 [100] ≤4.0 [100] ≤4.0 [100] ≤3.0 [75] >3 ≤5 [>75 ≤125] ≤3.0 [75]
45/15 [310/103] 45/15 [310/103] 45/15 [310/103] 50/20 [345/138] 50/18 [345/123] 50/20 [345/138]
Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet Plate & Sheet
71.5Cu-28Zn-1Sn-0.04Ag 71.5Cu-28Zn-1Sn-0.06Sb 71.5Cu-28Zn-1Sn-0.06P 60.5Cu-38Zn-0.75Sn 60.5Cu-38Zn-0.75Sn 60.5Cu-38Zn-0.75Sn-0.04Ag
C46500
>3 ≤5 [>75 ≤125] 50/18 [345/123]
Plate & Sheet
60.5Cu-38Zn-0.75Sn-0.04Ag
C36500
C23000 C44300 C44400 C44500 C68700
— — — — —
40/12 [276/83] 45/15 [310/103] 45/15 [310/103] 45/15 [310/103] 50/18 [345/123]
Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube
85Cu-15Zn 71.5Cu-28Zn-1Sn-0.04As 71.5Cu-28Zn-1Sn-0.06Sb 71.5Cu-28Zn-1Sn-0.06P 77.5Cu-31Zn-1.9Al-0.04As
C23000 C44300 C44400 C44500 C68700
— — — — —
40/12 [276/83] 45/15 [310/103] 45/15 [310/103] 45/15 [310/103] 50/18 [345/123]
Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube
85Cu-15Zn 71.5Cu-28Zn-1Sn-0.04Ag 71.5Cu-28Zn-1Sn-0.06Sb 71.5Cu-28Zn-1Sn-0.06P 67.5Cu-31Zn-1.9Al-0.04Ag
C23000 C44300
— —
40/12 [276/83] 45/15 [310/103]
Welded Tube Welded Tube
85Cu-15Zn 71.5Cu-28Zn-1Sn-0.04Ag
(Continued)
AWS B2.1/B2.1M-BMG:2009
32 32
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
148
32 32 32
ASTM ASTM ASTM
B 543 B 543 B 543
Admiralty, B Admiralty, C Aluminum Brass B
C44400 C44500 C68700
— — —
45/15 [310/103] 45/15 [310/103] 50/18 [345/123]
Welded Tube Welded Tube Welded Tube
71.5Cu-28Zn-1Sn-0.06Sb 71.5Cu-28Zn-1Sn-0.06P 67.5Cu-31Zn-1.9Al-0.04Ag
33 33 33 33 33 33 33 33 33 33 33
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 96 B 96 B 96 B 98 B 98 B 98 B 283 B 315 B 315 B 315 B 315
Low Si Bronze B Silicon Bronze High Si Bronze A Low Si Bronze B High Si Bronze A Silicon Bronze High Si Bronze A Low Si Bronze B High Si Bronze A Low Si Bronze B High Si Bronze A
C65100 C65400 C65500 C65100 C65500 C66100 C65500 C65100 C65500 C65100 C65500
— — — — — — — — — — —
38/– [262/–] 65/– [448/–] 52/– [359/–] 40/12 [276/83] 52/15 [359/103] 52/15 [359/103] 50/15 [345/103] 40/10 [276/69] 50/15 [345/103] 40/10 [276/69] 50/15 [345/103]
Plate, Sheet, Strip & Rolled Bar Plate, Sheet, Strip & Rolled Bar Plate, Sheet, Strip & Rolled Bar Rod, Bars & Shapes Rod, Bars & Shapes Rod, Bars & Shapes Die Forgings Pipe Pipe Tube Tube
96Cu-0.14Si 95Cu-3Si-1.5Sn 93Cu-3.3Si-0.9Mn 96Cu-0.14Si 93Cu-3.3Si-0.9Mn 93Cu-3.15Si-0.5Pb 93Cu-3.3Si-0.9Mn 96Cu-0.14Si 93Cu-3.3Si-0.9Mn 96Cu-0.14Si 93Cu-3.3Si-0.9Mn
34 34 34 34 34 34 34 34 34 34 34 34
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 111 B 111 B 111 B 111 B 111 B 111 B 151 B 151 B 151 B 151 B 151 B 171
95-5 Cu-Ni 90-10 Cu-Ni 80-20 Cu-Ni 70-30 Cu-Ni Cu-Ni-Fe-Mn 85-15 Cu-Ni 90-10 Cu-Ni 70-30 Cu-Ni 70-30 Cu-Ni 70-30 Cu-Ni 70-30 Cu-Ni 90-10 Cu-Ni
C70400 C70600 C71000 C71500 C71640 C72200 C70600 C71500 C71500 C71500 C71500 C70600
— — — — — — — ≤1/2 [13] >1/2 ≤1 [>13 ≤25] >1.0 [25] — —
38/12 [262/83] Seamless Tube & Ferrule Stock 40/15 [276/103] Seamless Tube & Ferrule Stock 45/16 [310/110] Seamless Tube & Ferrule Stock 52/18 [359/124] Seamless Tube & Ferrule Stock 63/25 [434/172] Seamless Tube & Ferrule Stock 45/16 [310/110] Seamless Tube & Ferrule Stock 38/15 [262/103] Rod, Bars & Shapes 52/18 [359/124] Round, Hex. & Oct. Rods & Square Bar 48/18 [331/124] Round, Hex. & Oct. Rods & Square Bar 45/18 [310/124] Round, Hex. & Oct. Rods & Square Bar 45/15 [310/103] Rectangular Bars & Shapes 40/15 [276/103] Plate & Sheet
(Continued)
92Cu-5.5Ni-1.5Fe-0.55Mn 87Cu-10Ni-1.4Fe 78Cu-21Ni-0.75Fe 68Cu-31Ni-0.7Fe 65Cu-30.5Ni-2Fe-2Mn 82Cu-16.5Ni-0.75Fe-0.5Cr 87Cu-10Ni-1.4Fe 68Cu-31Ni-0.7Fe 68Cu-31Ni-0.7Fe 68Cu-31Ni-0.7Fe 68Cu-31Ni-0.7Fe 87Cu-10Ni-1.4Fe
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
50/20 [345/138] 45/18 [310/124]
Plate & Sheet Plate & Sheet
68Cu-31Ni-0.7Fe 68Cu-31Ni-0.7Fe
42/16 [290/110] 38/12 [262/83] 40/15 [276/103] 45/16 [310/110] 52/18 [359/124] 45/16 [310/110] 38/12 [262/83] 40/15 [276/103] 45/16 [310/110] 52/18 [359/124] 45/16 [310/110] 37/12 [255/83] 38/13 [262/90] 45/16 [310/110] 52/18 [359/124] 40/14 [276/97] 40/15 [276/103] 38/13 [262/90] 50/20 [345/138] 45/15 [310/103] 38/12 [262/83] 40/15 [276/103] 45/16 [310/110] 52/18 [359/124] 63/25 [434/172] 45/16 [310/110]
Plate & Sheet Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
82Cu-16.5Ni-0.75Fe-0.5Cr 92Cu-5.5Ni-1.5Fe-0.55Mn 87Cu-10Ni-1.4Fe 78Cu-21Ni-0.75Fe 68Cu-31Ni-0.7Fe 82Cu-16.5Ni-0.75Fe-0.5Cr 92Cu-5.5Ni-1.5Fe-0.55Mn 87Cu-10Ni-1.4Fe 78Cu-21Ni-0.75Fe 68Cu-31Ni-0.7Fe 82Cu-16.5Ni-0.75Fe-0.5Cr 92Cu-5.5Ni-1.5Fe-0.55Mn 87Cu-10Ni-1.4Fe 78Cu-21Ni-0.75Fe 68Cu-31Ni-0.7Fe 82Cu-16.5Ni-0.75Fe-0.5Cr 87Cu-10Ni-1.4Fe 87Cu-10Ni-1.4Fe 68Cu-31Ni-0.7Fe 68Cu-31Ni-0.7Fe 92Cu-5.5Ni-1.5Fe-0.55Mn 87Cu-10Ni-1.4Fe 78Cu-21Ni-0.75Fe 68Cu-31Ni-0.7Fe 65Cu-30Ni-2Fe-2Mn 82Cu-16.5Ni-0.75Fe-0.5Cr
Copper and Copper Base Alloys
149
ASTM ASTM
B 171 B 171
70-30 Cu-Ni 70-30 Cu-Ni
C71500 C71500
34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34 34
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 171 B 359 B 359 B 359 B 359 B 359 B 395 B 395 B 395 B 395 B 395 B 466 B 466 B 466 B 466 B 466 B 467 B 467 B 467 B 467 B 543 B 543 B 543 B 543 B 543 B 543
85-15 Cu-Ni 95-5 Cu-Ni 90-10 Cu-Ni 80-20 Cu-Ni 70-30 Cu-Ni 85-15 Cu-Ni 95-5 Cu-Ni 90-10 Cu-Ni 80-20 Cu-Ni 70-30 Cu-Ni 85-15 Cu-Ni 95-5 Cu-Ni 90-10 Cu-Ni 80-20 Cu-Ni 70-30 Cu-Ni 85-15 Cu-Ni 90-10 Cu-Ni 90-10 Cu-Ni 70-30 Cu-Ni 70-30 Cu-Ni 95-5 Cu-Ni 90-10 Cu-Ni 80-20 Cu-Ni 70-30 Cu-Ni Cu-Ni-Fe-Mn 85-15 Cu-Ni
C72200 C70400 C70600 C71000 C71500 C72200 C70400 C70600 C71000 C71500 C72200 C70400 C70600 C71000 C71500 C72200 C70600 C70600 C71500 C71500 C70400 C70600 C71000 C71500 C71640 C72200
≤2.5 [64] >2.5 ≤5.0 [>64 ≤125] ≤2.5 [64] — — — — — — — — — — — — — — — ≤4.5 [114] >4.5 [114] ≤4.5 [114] >4.5 [114] — — — — — —
(Continued)
AWS B2.1/B2.1M-BMG:2009
34 34
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
150
34 34
ASTM ASTM
B 608 B 608
90-10 Cu-Ni 70-30 Cu-Ni
C70620 C71520
— —
40/– [276/–] 50/– [345/–]
Welded Pipe Welded Pipe
87Cu-10Ni-1.4Fe 68Cu-31Ni-0.7Fe
35
ASTM
B 111
C60800
—
50/19 [345/131]
Seamless Tube & Ferrule Stock
94Cu-5.8Al-0.2As
35
ASTM
B 111
C61300
—
70/30 [483/207]
Seamless Tube & Ferrule Stock
91Cu-6.8Al-2.5Fe-0.35Sn
35
ASTM
B 111
C61400
—
70/30 [483/207]
Seamless Tube & Ferrule Stock
87Cu-7.0Al-2.5Fe
35
ASTM
B 148
C95200
—
65/25 [448/172]
Sand Castings
88Cu-9Al-3Fe
35
ASTM
B 148
C95300
—
65/25 [448/172]
Sand Castings
89Cu-10Al-1Fe
35
ASTM
B 148
C95400
—
75/30 [517/207]
Sand Castings
85Cu-11Al-4Fe
35
ASTM
B 148
C95410
—
75/30 [517/207]
Sand Castings
83Cu-10.7Al-4Fe-2Ni
35
ASTM
B 148
C95500
—
90/40 [621/276]
Sand Castings
85Cu-11Al-4Fe-3Mn
35
ASTM
B 148
C95600
—
60/28 [414/193]
Sand Castings
91Cu-7Al-2Si
35
ASTM
B 148
C95700
—
90/40 [621/276]
Sand Castings
75Cu-12Mn-8Al-3Fe-2Ni
35 35
ASTM ASTM
B 148 B 150
C95800 C61300
— ≤0.50 [13]
85/35 [586/241] 80/40 [552/276]
Sand Castings Hex. & Oct. Rod & Bar
81Cu-9Al-4.5Ni-4Fe 90Cu-6.8Al-2.5Fe-0.35Sn
35
ASTM
B 150
C61300
Hex. & Oct. Rod & Bar
90Cu-6.8Al-2.5Fe-0.35Sn
ASTM
B 150
70/32 [483/221]
Hex. & Oct. Rod & Bar
90Cu-6.8Al-2.5Fe-0.35Sn
35
ASTM
B 150
>0.5 ≤1.0 [>13 ≤25] >1.0 ≤2.0 [>25 ≤50] ≤0.50 [13]
75/35 [517/241]
35
Aluminum Bronze Aluminum Bronze Aluminum Bronze D Grade A, AlBronze Grade B, AlBronze Grade C, AlBronze Aluminum Bronze Grade D, Ni-Al Bronze Grade E, Si-Al Bronze Grade F, Mn-NiAl Bronze Ni-Al Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze
80/50 [552/345]
Round Rod
90Cu-6.8Al-2.5Fe-0.35Sn
C61300 C61300
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
151
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze D Aluminum Bronze D Aluminum Bronze D Aluminum Bronze D Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze
>0.5 ≤1.0 [>13 ≤25] >1.0 ≤2.0 [>25 ≤50] >2.0 ≤3.0 [>50 ≤75] ≤0.5 [13]
75/45 [517/310]
Round Rod
90Cu-6.8Al-2.5Fe-0.35Sn
72/40 [496/276]
Round Rod
90Cu-6.8Al-2.5Fe-0.35Sn
70/35 [483/241]
Round Rod
90Cu-6.8Al-2.5Fe-0.35Sn
80/40 [552/276]
Round Rod
90Cu-7Al-2.5Fe
>0.5 ≤1.0 [>13 ≤25] >1.0 ≤2.0 [>25 ≤50] >2.0 ≤3.0 [>50 ≤75] ≤0.5 [13]
75/35 [517/241]
Round Rod
90Cu-7Al-2.5Fe
70/32 [483/221]
Round Rod
90Cu-7Al-2.5Fe
70/30 [483/207]
Round Rod
90Cu-7Al-2.5Fe
90/50 [621/345]
Round Rod
86Cu-9Al-3.7Fe
88/44 [607/303]
Round Rod
86Cu-9Al-3.7Fe
85/40 [586/276]
Round Rod
86Cu-9Al-3.7Fe
78/37 [538/255]
Round Rod
86Cu-9Al-3.7Fe
C61900
>0.5 ≤1.0 [>13 ≤25] >1.0 ≤2.0 [>25 ≤50] >2.0 ≤3.0 [>50 ≤75] >3.0 [>75]
75/30 [517/207]
Round Rod
86Cu-9Al-3.7Fe
C61900
—
75/30 [517/207]
Shapes
86Cu-9Al-3.7Fe
C62300
<0.5 [13]
90/50 [621/345]
Round Rod
86Cu-9.7Al-3Fe
C62300
>0.5 ≤1.0 [>13 ≤25] >1.0 ≤2.0 [>25 ≤50]
88/44 [607/303]
Round Rod
86Cu-9.7Al-3Fe
84/40 [579/276]
Round Rod
86Cu-9.7Al-3Fe
C61300 C61300 C61300 C61400 C61400 C61400 C61400 C61900 C61900 C61900 C61900
C62300
(Continued)
AWS B2.1/B2.1M-BMG:2009
35
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
152
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze
76/37 [524/255]
Round Rod
86Cu-9.7Al-3Fe
C62300
>2.0 ≤3.0 [>50 ≤75] >3.0 [75]
75/30 [517/207]
Round Rod
86Cu-9.7Al-3Fe
C62300
≤1.0 [25]
80/35 [552/241]
Hex. & Oct. Rod & Bar
86Cu-9.7Al-3Fe
C62300
78/32 [538/221]
Hex. & Oct. Rod & Bar
86Cu-9.7Al-3Fe
C62300
>1.0 ≤2.0 [>25 ≤50] >2.0 [50]
75/30 [517/207]
Hex. & Oct. Rod & Bar
86Cu-9.7Al-3Fe
C62300
—
75/30 [517/207]
Shapes
86Cu-9.7Al-3Fe
C62400
≤1.0 [25]
95/45 [655/310]
Round Rod
85.5Cu-10.8Al-3.2Fe
C62400
>1.0 ≤2.0 [>25 ≤50] >2.0 ≤3.0 [>50 ≤75] >3.0 ≤5.0 [>75 ≤125] 0.5 ≤5.0 [13 ≤125] —
90/43 [621/296]
Round Rod
85.5Cu-10.8Al-3.2Fe
90/40 [621/276]
Round Rod
85.5Cu-10.8Al-3.2Fe
90/35 [621/241]
Round Rod
85.5Cu-10.8Al-3.2Fe
90/35 [621/241]
Hex. & Oct. Rod & Bar
85.5Cu-10.8Al-3.2Fe
90/35 [621/241]
Shapes
85.5Cu-10.8Al-3.2Fe
0.5 ≤1.0 [13 ≤25] >1.0≤ 2.0 [>25 ≤50] >2.0 ≤4.0 [>50 ≤100] >4.0 [100]
100/50 [689/345]
Rod & Bar
82Cu-10Al-5Ni-3Fe
90/45 [621/310]
Rod & Bar
82Cu-10Al-5Ni-3Fe
85/42.5 [586/293]
Rod & Bar
82Cu-10Al-5Ni-3Fe
80/40 [552/276]
Rod & Bar
82Cu-10Al-5Ni-3Fe
C62300
C62400 C62400 C62400 C62400 C63000 C63000 C63000 C63000
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
153
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 150
35
ASTM
B 169
35
ASTM
B 169
35
ASTM
B 169
35
ASTM
B 169
Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze D
C63000
—
85/42.5 [586/293]
Shapes
82Cu-10Al-5Ni-3Fe
C63020
≤1.0 [25]
135/100 [931/689]
Rod & Bar
74.5minCu-11Al-5.1Ni-4.8Fe
C63020
130/95 [896/655]
Rod & Bar
74.5minCu-11Al-5.1Ni-4.8Fe
130/90 [896/621]
Rod & Bar
74.5minCu-11Al-5.1Ni-4.8Fe
C63200
>1.0 ≤2.0 [>25 ≤50] >2.0 ≤4.0 [>50 ≤100] —
90/40 [621/276]
Rod, Bars & Shapes
C64200
≤0.5 [13]
90/45 [621/310]
Rod & Bar
81Cu-9.1Al-4.4Ni-3.9Fe1.6Mn 89Cu-6.9Al-1.8Si
C64200
>0.5 ≤1.0
85/45 [586/310]
Rod & Bar
89Cu-6.9Al-1.8Si
C64200
80/42 [552/290]
Rod & Bar
89Cu-6.9Al-1.8Si
75/35 [517/241]
Rod & Bar
89Cu-6.9Al-1.8Si
70/30 [483/207]
Rod & Bar
89Cu-6.9Al-1.8Si
C64200
>1.0 ≤2.0 [>25 ≤50] >2.0 ≤3.0 [>50 ≤75] >3.0 ≤4.0 [>75 ≤100] >4.0 [100]
70/25 [483/172]
Rod & Bar
89Cu-6.9Al-1.8Si
C64200
—
70/30 [483/207]
Shapes
89Cu-6.9Al-1.8Si
C61300
≤0.5 [13]
75/36 [517/248]
Sheet, Strip & Rolled Bar
90Cu-6.8Al-2.5Fe-0.35Sn
C61300
>0.5 ≤2.0 [>13 ≤50] >2.0 ≤5.0 [>50 ≤125] ≤0.5 [13]
72/32 [496/221]
Sheet, Strip & Rolled Bar
90Cu-6.8Al-2.5Fe-0.35Sn
65/28 [448/193]
Sheet, Strip & Rolled Bar
90Cu-6.8Al-2.5Fe-0.35Sn
72/32 [496/221]
Sheet, Strip & Rolled Bar
90Cu-7Al-2.5Fe
C63020
C64200 C64200
C61300 C61400
(Continued)
AWS B2.1/B2.1M-BMG:2009
35
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
154
35
ASTM
B 169
35
ASTM
B 169
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 171
35
ASTM
B 271
35
ASTM
B 271
35
ASTM
B 271
Aluminum Bronze D Aluminum Bronze D Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze D Aluminum Bronze D Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Aluminum Bronze Grade A, AlBronze Grade B, AlBronze Grade C, AlBronze
>0.5 ≤2.0 [>13 ≤50] >2.0 ≤5.0 [>50 ≤125] ≤2.0 [50]
70/30 [483/207]
Sheet, Strip & Rolled Bar
90Cu-7Al-2.5Fe
65/28 [448/193]
Sheet, Strip & Rolled Bar
90Cu-7Al-2.5Fe
75/37 [517/255]
Plate & Sheet
90Cu-6.8Al-2.5Fe-0.35Sn
>2.0 ≤3.0 [>50 ≤75] >3.0 ≤5.0 [>75 ≤125] ≤2.0 [50]
70/30 [483/207]
Plate & Sheet
90Cu-6.8Al-2.5Fe-0.35Sn
65/28 [448/193]
Plate & Sheet
90Cu-6.8Al-2.5Fe-0.35Sn
70/30 [483/207]
Plate & Sheet
90Cu-7Al-2.5Fe
>2.0 ≤5.0 [>50 ≤125] ≤2.0 [50]
65/28 [448/193]
Plate & Sheet
90Cu-7Al-2.5Fe
90/36 [621/248]
Plate & Sheet
82Cu-10Al-5Ni-3Fe
>2.0 ≤3.5 [>50 ≤89] >3.5 ≤5.0 [>89 ≤125] ≤2.0 [50]
85/33 [586/228]
Plate & Sheet
82Cu-10Al-5Ni-3Fe
80/30 [552/207]
Plate & Sheet
82Cu-10Al-5Ni-3Fe
90/36 [621/248]
Plate & Sheet
85/33 [586/228]
Plate & Sheet
80/30 [552/207]
Plate & Sheet
C95200
>2.0 ≤3.5 [>50 ≤89] >3.5 ≤5.0 [>89 ≤125] —
65/25 [448/172]
Centrifugal Castings
81Cu-9.1Al-4.4Ni-3.9Fe1.6Mn 81Cu-9.1Al-4.4Ni-3.9Fe1.6Mn 81Cu-9.1Al-4.4Ni-3.9Fe1.6Mn 88Cu-9Al-3Fe
C95300
—
65/25 [448/172]
Centrifugal Castings
89Cu-10Al-1Fe
C95400
—
75/30 [517/207]
Centrifugal Castings
85Cu-11Al-4Fe
C61400 C61400 C61300 C61300 C61300 C61400 C61400 C63000 C63000 C63000 C63200 C63200 C63200
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Base Metal Type, Grade, or Number Standard Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Copper and Copper Base Alloys
155
35
ASTM
B 271
35
ASTM
B 271
35 35 35
ASTM ASTM ASTM
B 283 B 283 B 315
35
ASTM
B 315
35
ASTM
B 359
35
ASTM
B 395
35
ASTM
B 505
35
ASTM
B 608
35
ASTM
B 608
Aluminum Bronze Grade D, Ni-Al Bronze Al-Si Bronze Al-Si Bronze Aluminum Bronze Aluminum Bronze D Aluminum Bronze Aluminum Bronze Grade A, AlBronze Aluminum Bronze Aluminum Bronze D
C95410
—
75/30 [517/207]
Centrifugal Castings
83Cu-10.7Al-4Fe-2Ni
C95500
—
90/40 [621/276]
Centrifugal Castings
85Cu-11Al-4Fe-3Mn
C64200 C64200 C61300
≤1.5 [38] >1.5 [38] —
70/25 [483/172] 68/23 [469/159] 65/28 [448/193]
Die Forgings Die Forgings Seamless Pipe
89Cu-7Al-1.8Si 89Cu-7Al-1.8Si 90Cu-6.8Al-2.5Fe-0.35Sn
C61400
—
65/28 [448/193]
Seamless Pipe
90Cu-7Al-2.5Fe
C60800
—
50/19 [345/131]
Seamless Tube
93.5Cu-5.8Al-0.27As
C60800
—
50/19 [345/131]
Seamless Tube
93.5Cu-5.8Al-0.27As
C95200
20% of t
68/– [469/–]
Continuous Casting Repair
80Cu-9Al-3Fe
C61300
—
70/– [483/–]
Welded Pipe
90Cu-6.8Al-2.5Fe-0.35Sn
C61400
—
70/– [483/–]
Welded Pipe
90Cu-7Al-2.5Fe
AWS B2.1/B2.1M-BMG:2009
Material Base Metal Number Standard Specification
Thickness or Diameter Limitations, in [mm]
Type, Grade, or Alloy Designation
UNS Number
N02200 N02201
— —
N02200 N02200 N02201
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
55/15 [379/103] 50/10 [345/69]
Rod & Bar Rod & Bar
99.0min.Ni LoC-99min.Ni
≤5 [125] O.D. >5 [125] O.D. ≤5 [125] O.D.
55/15 [379/103] 55/12 [379/83] 50/12 [345/83]
Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube
99.0min.Ni 99.0min.Ni LoC-99min.Ni
N02201
>5 [125] O.D.
50/10 [345/69]
Seamless Pipe & Tube
LoC-99min.Ni
N02200 N02201
— —
55/15 [379/103] 50/12 [345/83]
Sheet, Strip & Plate Sheet, Strip & Plate
99.0min.Ni LoC-99min.Ni
N02200 N02201
— —
55/15 [379/103] 50/12 [345/83]
Seamless Tube Seamless Tube
99.0min.Ni LoC-99min.Ni
N02200 N02201 N02200
— — —
55/15 [379/103] 50/10 [345/69] 55/15 [379/103]
Fittings Fittings Forgings
99.0min.Ni LoC-99min.Ni 99.0min.Ni
N04020 N24130 N24135 N04400 N04400 N04400 N04405 N04400 N04400 N04400 N04400
— — — — — — — ≤5 [125] O.D. >5 [125] O.D. — —
65/30 [448/207] 65/32 [448/221] 65/25 [448/172] 70/28 [483/193] 70/28 [483/193] 70/25 [483/172] 70/25 [483/172] 70/28 [483/193] 70/25 [483/172] 70/25 [483/172] 70/25 [483/172]
Castings Castings Castings Sheet, Strip & Plate Seamless Tube Rod, Bar & Wire Rod, Bar & Wire Seamless Pipe & Tube Seamless Pipe & Tube Fittings Forgings
67Ni-31Cu 66Ni-30Cu-2Cb 67Ni-3Cu 67Ni-31Cu 67Ni-31Cu 67Ni-31Cu 67Ni-30Cu-S 67Ni-31Cu 67Ni-31Cu 67Ni-31Cu 67N-31Cu
Nickel and Nickel Base Alloys
156
41 41
ASTM ASTM
B 160 B 160
41 41 41
ASTM ASTM ASTM
B 161 B 161 B 161
41
ASTM
B 161
41 41
ASTM ASTM
B 162 B 162
41 41
ASTM ASTM
B 163 B 163
41 41 41
ASTM ASTM ASTM
B 366 B 366 B 564
99.0 min. Ni (Alloy 200) Low-C 99 min. Ni (Alloy 201) 99.0 min. Ni (Alloy 200) 99.0 min. Ni (Alloy 200) Low-C 99 min. Ni (Alloy 201) Low-C 99 min. Ni (Alloy 201) 99.0 min. Ni (Alloy 200) Low-C 99 min. Ni (Alloy 201) 99.0 min. Ni (Alloy 200) Low-C 99 min. Ni (Alloy 201) CRN/WPN CRNL/WPNL Alloy 200
42 42 42 42 42 42 42 42 42 42 42
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 494 A 494 A 494 B 127 B 163 B 164 B 164 B 165 B 165 B 366 B 564
Grade M-35-2 (Ni-30 Cu) Grade M-30-C Grade M-35-1 Ni-Cu (30) (Alloy 400) Ni-Cu (30) (Alloy 400) Ni-Cu (30) (Alloy 400) Ni-Cu (30) (Alloy R 405) Ni-30Cu (Alloy 400) Ni-30Cu (Alloy 400) CRNC/WPNC Alloy 400
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
70/28 [483/193] 80/45 [552/310] 72/40 [496/276] 70/40 [483/276] 72/40 [496/276] 98/39 [676/269] 80/35 [552/241] 85/35 [586/241] 98/39 [676/269] 80/35 [552/241] 80/30 [552/207] 95/35 [655/241] 85/35 [586/241] 98/39 [676/269] 80/30 [552/207]
Castings Castings Castings Castings Castings Seamless Tube Seamless Tube Seamless Tube Rod & Bar Rod & Bar Rod & Bar Rod & Bar Rod & Bar Seamless Pipe & Tube Seamless Pipe & Tube
77Ni-15.5Cr-Fe 57Ni-21Cr-13Mo-4Fe-3W 65.6Ni-16.2Cr-16.2Mo 62Ni-21.5Cr-9Mo-4Cb 61Ni-18.5Cr-18.5Mo-Fe 62.5Ni-25Cr-9.5Fe-2.1Al 72Ni-15Cr-8Fe 58Ni-29Cr-9Fe 62.5Ni-25Cr-9.5Fe-2.1Al 72Ni-15Cr-8Fe 60Ni-23Cr-12Fe-Al 54Ni-22Cr-12Co-9Mo 58Ni-29Cr-9Fe 62.5Ni-25Cr-9.5Fe-2.1Al 75Ni-15Cr-8Fe
75/25 [517/172]
Seamless Pipe & Tube
75Ni-15Cr-8Fe
80/30 [552/207]
Seamless Pipe & Tube
60Ni-23Cr-12Fe-Al
85/30 [586/207]
Seamless Pipe & Tube
58Ni-29Cr-9Fe
75/25 [517/172]
Seamless Pipe & Tube
58Ni-29Cr-9Fe
98/39 [676/269] 80/35 [552/241] 80/30 [552/207] 95/35 [655/241] 85/35 [586/241] 100/– [689/–]
Sheet, Strip & Plate Sheet, Strip & Plate Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Fittings
62.5Ni-25Cr-9.5Fe-2.1Al 75Ni-15Cr-8Fe 60Ni-23Cr-12Fe-Al 54Ni-22Cr-12Co-9Mo 58Ni-29Cr-9Fe 47Ni-22Cr-18Fe-9Mo
Nickel and Nickel Base Alloys
157
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
A 494 A 494 A 494 A 494 A 494 B 163 B 163 B 163 B 166 B 166 B 166 B 166 B 166 B 167 B 167
Grade CY-40 Grade CX2MW Grade CW2M Grade CW-6 MC Grade CW-6M Ni-Cr-Fe (Alloy 6025HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe (Alloy 6025 HT) Ni-Cr-Fe (Alloy 600) Ni-Cr-Fe (Alloy 601) Ni-Cr-Co-Mo (Alloy 617) Ni-Cr-Fe (Alloy 690) Ni-Cr-Fe (Alloy 6025HT) Ni-Cr-Fe (Alloy 600)
N06040 N26022 N26455 N26625 N30107 N06025 N06600 N06690 N06025 N06600 N06601 N06617 N06690 N06025 N06600
43
ASTM
B 167
Ni-Cr-Fe (Alloy 600)
N06600
43
ASTM
B 167
Ni-Cr-Fe (Alloy 601)
N06601
43
ASTM
B 167
Ni-Cr-Fe (Alloy 690)
N06690
43
ASTM
B 167
Ni-Cr-Fe (Alloy 690)
N06690
43 43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM ASTM
B 168 B 168 B 168 B 168 B 168 B 366
Alloy 6025 HT Alloy 600 Alloy 601 Alloy 617 Alloy 690 CRHX/WPHX
N06025 N06600 N06601 N06617 N06690 N06002
— — — — — — — — — — — — — — 0.405 ≤5 [10.29 ≤125] O.D. >5.0 ≤9.25 [125 ≤235] O.D. 0.405 ≤9.25 [10.29 ≤235] O.D. 0.405 ≤5 [10.29 ≤125] O.D >5.0 ≤9.25 [125 ≤235] O.D. — — — — — —
(Continued)
AWS B2.1/B2.1M-BMG:2009
43 43 43 43 43 43 43 43 43 43 43 43 43 43 43
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Nickel and Nickel Base Alloys
158
43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 435 B 435 B 443 B 443
CRHG/WPHG CRHC22/WPHC22 CRV602/WPV602 CRHG30/WPHG30 CR5923/WP5923 CRHC2000/WPHC2000 CRM21/WPM21 CRH230/WPH230 CRHC4/WPHC4 CRNCI/WPNCI CR603GT/WP603GT CRNCMC/WPNCMC CRHG3/WPHG3 CRHC276/WPHC276 Alloy X Alloy 230 Alloy 625, Grade 1 Alloy 625, Grade 2
N06007 N06022 N06025 N06030 N06059 N06200 N06210 N06230 N06455 N06600 N06603 N06625 N06985 N10276 N06002 N06230 N06625 N06625
— — — — — — — — — — — — — — — — — —
90/– [621/–] 100/45 [689/310] 98/39 [676/269] 85/35 [586/241] 85/35 [586/241] 100/41 [689/283] 100/45 [689/310] 110/45 [758/310] 100/40 [689/276] 80/– [552/–] 94/43 [648/296] 110/– [758/–] 90/– [621/–] 100/41 [689/283] 95/35 [655/241] 110/45 [758/310] 120/60 [827/414] 110/55 [758/379]
47Ni-22Cr-19Fe-6Mo 55Ni-21Cr-13.5Mo 60Ni-22Cr-9Mo-3.5Cb 40Ni-29Cr-15Fe-5Mo 59Ni-23Cr-16Mo 58Ni-23Cr-16Mo-1.6Cu 59Ni-19Cr-19Mo-1.8Ta 56Ni-22Cr-14W-2Mb 65Ni-10Cr-15.5Mo 75Ni-15Cr-8Fe 62Ni-25Cr-9Fe-2.7Al 60Ni-22Cr-9Mo-3.5Cb 47Ni-22Cr-20Fe-7Mn 54Ni-16Mo-15Cr-5.5Fe-3.8W 47Ni-22Cr-18Fe-9Mo 53Ni-22Cr-14W-2Mo 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb
120/60 [827/414] 100/40 [689/276] 120/60 [827/414] 110/50 [758/345]
Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Plate, Sheet & Strip Plate, Sheet & Strip Cold Rolled Strip & Sheet Plate & Hot Rolled Sheet (Sol. Anneal) Pipe & Tube Pipe & Tube Rod & Bar Rod & Bar
43 43 43 43
ASTM ASTM ASTM ASTM
B 444 B 444 B 446 B 446
Alloy 625, Grade 1 Alloy 625, Grade 2 Alloy 625, Grade 1 Alloy 625, Grade 1
N06625 N06625 N06625 N06625
43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM
B 446 B 516 B 516 B 516 B 517
Alloy 625, Grade 2 Alloy 6025 HT Alloy 600 Alloy 603 GT Alloy 6025 HT
N06625 N06025 N06600 N06603 N06025
— — ≤4 [100] >4 ≤10 [>100 ≤250] — — — — —
110/40 [758/276] 98/39 [676/269] 80/35 [552/241] 94/43 [648/296] 98/39 [676/269]
Rod & Bar Welded Tube Welded Tube Welded Tube Welded Pipe
60Ni-22Cr-9Mo-3.5Cb 62.5Ni-25Cr-9.5Fe-2.1Al 75Ni-15Cr-8Fe 62Ni-25Cr-9Fe-2.7Al 62.5Ni-25Cr-9.5Fe-2.1Al
(Continued)
60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Welded Pipe Welded Pipe Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Rod Rod Rod Rod Rod Rod Rod Rod Plate, Sheet & Strip
75Ni-15Cr-8Fe 62Ni-25Cr-9Fe-2.7Al 56Ni-21Cr-13.5Mo 62.5Ni-25Cr-9.5Fe-2.1Al 62.5Ni-25Cr-9.5Fe-2.1Al 59Ni-23Cr-16Mo 51Ni-31Cr-10Mo-W 51Ni-31Cr-10Mo-W 53Ni-23Cr-16Mo-1.6Cu 60Ni-19Cr-19Mo-1.8Ta 53Ni-22Cr-14W-2Mo 75Ni-15Cr-8Fe 62Ni-25Cr-9Fe-2.7Al 54Ni-22Cr-12Co-9Mo 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb 58Ni-21Cr-16Mo-3.7W 58Ni-29Cr-9Fe 54Ni-16Mo-15Cr-5.5Fe-3.8W 65Ni-22.5Mo-6.5Fe-6Cr 56Ni-22Cr-14W-2Mo 47Ni-22Cr-18Fe-9Mo 56Ni-21Cr-13.5Mo 59Ni-23Cr-16Mo 53Ni-23Cr-16Mo-1.6Cu 61Ni-16Mo-16Cr 58Ni-21Cr-16Mo-3.5W 54Ni-16Mo-15Cr-5.5Fe-3.8W 56Ni-21Cr-13.5Mo
Nickel and Nickel Base Alloys
159
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 517 B 517 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 572 B 572 B 574 B 574 B 574 B 574 B 574 B 574 B 575
Alloy 600 Alloy 603GT Alloy C-22 Alloy 6025 HT Alloy 6025 HT Alloy 59 Ni-Cr-Mo-W Ni-Cr-Mo-W Alloy C2000 Alloy 21 Alloy 230 Alloy 600 Alloy 603GT Alloy 617 Alloy 625 Alloy 625 Alloy 686 Alloy 690 Alloy C-276 Alloy CRB10 Alloy 230 Alloy X Alloy C22 Alloy 59 Alloy C2000 Alloy C-4 Alloy C686 Alloy C-276 Alloy C22
N06600 N06603 N06022 N06025 N06025 N06059 N06110 N06110 N06200 N06210 N06230 N06600 N06603 N06617 N06625 N06625 N06686 N06690 N10276 N10624 N06230 N06002 N06022 N06059 N06200 N06455 N06686 N10276 N06022
— — — ≤4 [100] >4 [100]
80/35 [552/241] 94/43 [648/296] 100/45 [689/310] 98/39 [676/269] 84/39 [579/269] 100/45 [689/310] ≤4 [100] 95/45 [655/310] >4.0 [100] 90/40 [621/276] — 100/41 [689/283] — 100/45 [689/310] — 110/45 [758/310] — 80/35 [552/241] — 94/43 [648/296] — 95/35 [655/241] ≤4 [100] 120/60 [827/414] >4.0 [100] 110/50 [758/345] — 100/45 [689/310] — 85/35 [586/241] — 100/41 [689/283] — 104/46 [717/317] — 110/45 [758/310] — 95/35 [655/241] — 100/45 [689/310] — 100/45 [689/310] — 100/41 [689/283] — 100/40 [689/276] — 100/45 [689/310] — 100/41 [689/283] — 100/45 [689/310] (Continued)
AWS B2.1/B2.1M-BMG:2009
43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
100/45 [689/310] 100/41 [689/283] 100/40 [689/276] 100/45 [689/310] 100/41 [689/283] 90/35 [621/241] 85/30 [586/207]
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Rod Rod
59Ni-23Cr-16Mo 53Ni-23Cr-16Mo-1.6Cu 61Ni-16Mo-16Cr 58Ni-21Cr-16Mo-3.5W 54Ni-16Mo-15Cr-5.5Fe-3.8W 47Ni-22Cr-19Fe-6Mo 47Ni-22Cr-19Fe-6Mo
85/35 [586/241] 85/32 [586/221] 90/35 [621/241] 85/30 [586/207]
Rod Rod Rod Rod
40Ni-29Cr-15Fe-5Mo 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-18Fe-6Mo 47Ni-22Cr-18Fe-6Mo
90/35 [621/241] 85/30 [586/207]
Plate, Sheet & Strip Plate
47Ni-22Cr-19Fe-6Mo 47Ni-22Cr-19Fe-6Mo
85/35 [586/241] 85/32 [586/221] 90/35 [621/241] 85/30 [586/207]
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate
40Ni-29Cr-15Fe-5Mo 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 47Ni-22Cr-20Fe-7Mo
100/40 [689/276] 90/35 [621/241] 100/45 [689/310] 85/35 [586/241] 100/45 [689/310] 100/41 [689/283] 110/45 [758/310] 100/40 [689/276]
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Pipe Welded Pipe
47Ni-22Cr-18Fe-9Mo 47Ni-22Cr-19Fe-6Mo 56Ni-21Cr-13.5Mo 40Ni-29Cr-15Fe-5Mo 59Ni-23Cr-16Mo 53Ni-23Cr-16Mo-1.6Cu 53Ni-22Cr-14W-2Mo 61Ni-16Mo-16Cr
Nickel and Nickel Base Alloys
160
43 43 43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 575 B 575 B 575 B 575 B 575 B 581 B 581
Alloy 59 Alloy C2000 Alloy C-4 Alloy 686 Alloy C-276 Alloy G Alloy G
N06059 N06200 N06455 N06686 N10276 N06007 N06007
43 43 43 43
ASTM ASTM ASTM ASTM
B 581 B 581 B 581 B 581
Alloy G-30 Alloy G-2 Alloy G-3 Alloy G-3
N06030 N06975 N06985 N06985
43 43
ASTM ASTM
B 582 B 582
Alloy G Alloy G
N06007 N06007
43 43 43 43
ASTM ASTM ASTM ASTM
B 582 B 582 B 582 B 582
Alloy G-30 Alloy G-2 Alloy G-3 Alloy G-3
N06030 N06975 N06985 N06985
43 43 43 43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 619 B 619 B 619 B 619 B 619 B 619 B 619 B 619
Alloy X Alloy G Alloy C-22 Alloy G-30 Alloy 59 Alloy C2000 Alloy 230 Alloy C-4
N06002 N06007 N06022 N06030 N06059 N06200 N06230 N06455
— — — — — 5/16 ≤3/4 [8 ≤19] >3/4 ≤3.5 [>19 ≤89] — — 5/16 ≤3/4 [8 ≤19] >3/4 ≤3.5 [>19 ≤89] 0.20 ≤3/4 [5 ≤19] >3/4 ≤2.5 [>19 ≤64] — — 0.20 ≤3/4 [5 ≤19] >3/4 ≤2.5 [>19 ≤64] — — — — — — — —
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Welded Pipe Welded Pipe Welded Pipe Welded Pipe Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
58Ni-21Cr-16Mo-3.5W 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 54Ni-16Mo-15Cr-5.5Fe-3.8W 47Ni-22Cr-18Fe-9Mo 47Ni-22Cr-19Fe-6Mo 56Ni-21Cr-13.5Mo 40Ni-29Cr-15Fe-5Mo 59Ni-23Cr-16Mo 57Ni-20.5Cr-13Mo-6Fe 53Ni-23Cr-16Mo-1.6Cu 53Ni-22Cr-14W-2Mo 52Ni-21Cr-13Fe-11Mo 49.5Ni-24Cr-17Fe-7Mo 58Ni-21Cr-16Mo-3.5W 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 54Ni-16Mo-15Cr-5.5Fe-3.8W — 47Ni-22Cr-19Fe-6Mo 56Ni-21Cr-13.5Mo 40Ni-29Cr-15Fe-5Mo 59Ni-23Cr-16Mo 53Ni-23Cr-16Mo-1.6Cu 59Ni-22Cr-14W-Fe-Mo 65.6Ni-16.2Cr-16.2Mo 58Ni-21Cr-16Mo-3.5W 49Ni-25Cr-18Fe-6Mo-Ti 47Ni-22Cr-20Fe-7Mo-2Cu
Nickel and Nickel Base Alloys
161
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 619 B 619 B 619 B 619 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 622 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626 B 626
Alloy 686 Alloy G-2 Alloy G-3 Alloy C-276 Alloy X Alloy G Alloy C-22 Alloy G-30 Alloy 59 Alloy 2060 Mo Alloy C2000 Alloy 230 Alloy 2050 Alloy 2550 Alloy 686 Alloy G-2 Alloy G-3 Alloy C-276 Ni-Cr-Fe-Mo Alloy G Alloy C-22 Alloy G30 Alloy 59 Alloy C2000 Alloy 230 Alloy C-4 Alloy 686 Alloy G-2 Alloy G-3
N06686 N06975 N06985 N10276 N06002 N06007 N06022 N06030 N06059 N06060 N06200 N06230 N06250 N06255 N06686 N06975 N06985 N10276 N06002 N06007 N06022 N06030 N06059 N06200 N06230 N06455 N06686 N06975 N06985
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
100/45 [689/310] 85/32 [586/221] 90/35 [621/241] 100/41 [689/283] 100/40 [689/276] 90/35 [621/241] 100/45 [689/310] 85/35 [586/241] 100/45 [689/310] 90/35 [621/241] 100/41 [689/283] 110/45 [758/310] 90/35 [621/241] 85/32 [586/221] 100/45 [689/310] 85/32 [586/221] 90/35 [621/241] 100/41 [689/283] — 90/35 [621/241] 100/45 [689/310] 85/35 [586/241] 100/45 [689/310] 100/41 [689/283] 110/45 [758/310] 100/40 [689/276] 100/45 [689/310] 85/32 [586/221] 90/32 [621/221] (Continued)
AWS B2.1/B2.1M-BMG:2009
43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43 43
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Nickel and Nickel Base Alloys
162
43 43 43 43 43 43
ASTM ASTM ASTM ASTM ASTM ASTM
B 626 B 704 B 705 B 755 B 756 B 756
Alloy C-276 Alloy 625 Alloy 625 Ni-Cr-Mo-W Ni-Cr-Mo-W Ni-Cr-Mo-W
N10276 N06625 N06625 N06110 N06110 N06110
43 43 43
ASTM ASTM ASTM
B 757 B 758 B 759
Ni-Cr-Mo-W Ni-Cr-Mo-W Ni-Cr-Mo-W
N06110 N06110 N06110
44 44 44
ASTM ASTM ASTM
A 494 B 333 B 333
Grade N7M Alloy B (Ni-Mo-Fe) Alloy B (Ni-Mo-Fe)
J30007 N10001 N10001
44 44 44 44 44 44 44 44 44 44 44 44 44 44
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 333 B 333 B 333 B 333 B 335 B 335 B 335 B 335 B 335 B 335 B 366 B 366 B 366 B 366
N10624 N10629 N10665 N10675 N10001 N10001 N10624 Alloy B-4 (Ni-Mo-Fe) N10629 Alloy B-2 (Ni-Mo) N10665 Alloy B-3 (Ni-Mo-Cr-Fe) N10675 CRHB/WPHB N10001 CRHN/WPHN N10003 CRB10/WPB10 N10624 CRVB4/WPVB4 N10629 Alloy B-4 (Ni-Mo-Fe) Alloy B-2 (Ni-Mo) Alloy B-3 (Ni-Mo-Cr-Fe) Alloy B (Ni-Mo-Fe) Alloy B (Ni-Mo-Fe)
— — — — ≤4 [100] >4.0≤10 [>100 ≤250] — — —
100/41 [689/283] 120/60 [827/414] 120/60 [827/414] 95/45 [655/310] 95/45 [655/310] 90/40 [621/276]
Welded Tube Welded Tube Welded Pipe Plate, Sheet & Strip Rod & Bar Rod & Bar
54Ni-16Mo-15Cr-5.5Fe-3.8W 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb 51Ni-31Cr-10Mo-2.5W 51Ni-31Cr-10Mo-2.5W 51Ni-31Cr-10Mo-2.5W
95/45 [655/310] 95/45 [655/310] 95/45 [655/310]
Welded Pipe Welded Tube Pipe & Tube
51Ni-31Cr-10Mo-2.5W 51Ni-31Cr-10Mo-2.5W 51Ni-31Cr-10Mo-2.5W
— ≤3/16 [5] 3/16 ≤ 2.5 [5 ≤64] — — — — 5/16 ≤1.5 [8 ≤38] >1.5 ≤2.5 [38 ≤64] — — — — — — — —
76/40 [524/276] 115/50 [793/345] 100/45 [689/310]
Castings Sheet & Strip Plate
61Ni-31.5Mo 62Ni-28Mo-5maxFe 62Ni-28Mo-5maxFe
104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 110/51 [758/352] 115/46 [793/317] 100/45 [689/310] 104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 110/51 [758/352] 100/45 [689/310] 100/– [689/–] 104/46 [717/317] 110/51 [758/352]
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Rod Rod Rod Rod Rod Rod Fittings Fittings Fittings Fittings
60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3Fe-1.3Cr-Al 65Min.Ni-28Mo-2Fe 65Ni-30Mo-2Cr-2Fe 62Ni-28Mo-5Max.Fe 62Ni-28Mo-5Max.Fe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3Fe-1.3Cr-Al 65Min.Ni-28Mo-2Fe-2C 65Ni-30Mo-2Cr-2Fe 62Ni-28Mo-5maxFe 70Ni-16Mo-7Cr-5Fe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3Fe-1.3Cr-Al
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Fittings Fittings Plate, Sheet & Strip Forgings Forgings Forgings Rod Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Welded Tube Welded Tube Welded Tube Welded Tube Welded Tube
65Ni-28Mo-2Max.Fe 65Min.Ni-29.5Mo-2Cr-2Fe 70Ni-16Mo-7Cr-5Fe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3.5Fe-1Cr 65Min.Ni-29.5Mo-2Cr-2Fe 70Ni-16Mo-7Cr-5Fe 62Ni-28Mo-5maxFe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3.5Fe-1Cr 65Ni-28Mo-2Max.Fe 65Min.Ni-29.5Mo-2Cr-2Fe 62Ni-28Mo-2Max.Fe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3.5Fe-1Cr 65Ni-28Mo-2Max.Fe 65Min.Ni-29.5Mo-2Cr-2Fe 62Ni-28Mo-5maxFe 60Ni-23Mo-8Cr-6.5Fe 62Ni-28Mo-3.5Fe-1Cr 65Ni-28Mo-2Max.Fe 65Min.Ni-29.5Mo-2Cr-2Fe
Castings Castings Seamless Tube Seamless Tube Seamless Tube Seamless Tube
43Fe-28Ni-19Cr-Cu-Mn 46Fe-32Ni-20Cr-Cb 44Fe-33Ni-21Cr 45Fe-32Ni-20.5Cr-Ti 44Fe-33Ni-21Cr 42Fe-33Ni-21Cr-Al-Ti
Nickel and Nickel Base Alloys
163
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 366 B 366 B 434 B 564 B 564 B 564 B 573 B 619 B 619 B 619 B 619 B 619 B 622 B 622 B 622 B 622 B 622 B 626 B 626 B 626 B 626 B 626
CRHB2/WPHB2 CRHB3/WPHB3 Alloy N Alloy B-10 Alloy B-4 (Ni-Mo-Fe) Alloy B-3 Alloy N Alloy B Alloy B-10 Alloy B-4 Alloy B-2 Alloy B-3 Alloy B Alloy B-10 Alloy B-4 Alloy B-2 Alloy B-3 Alloy B Alloy B-10 Alloy B-4 Alloy B-2 Alloy B-3
N10665 N10675 N10003 N10624 N10629 N10675 N10003 N10001 N10624 N10629 N10665 N10675 N10001 N10624 N10629 N10665 N10675 N10001 N10624 N10629 N10665 N10675
— — — — — — — — — — — — — — — — — — — — — —
100/– [689/–] 110/51 [758/352] 100/40 [689/276] 104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 100/40 [689/276] 100/45 [689/310] 104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 110/51 [758/352] 100/45 [689/310] 104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 110/51 [758/352] 100/45 [689/310] 104/46 [717/317] 110/51 [758/352] 110/51 [758/352] 110/51 [758/352]
45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM
A 351 A 351 B 163 B 163 B 163 B 163
CN7M CT15C Ni-Fe-Cr (Alloy 800) Ni-Fe-Cr (Alloy 801) Ni-Fe-Cr (Alloy 800H) Ni-Fe-Cr (Alloy 800HT)
N08007 N08151 N08800 N08801 N08810 N08811
— — — — — —
62/25 [427/172] 63/25 [434/172] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 65/25 [448/172] (Continued)
AWS B2.1/B2.1M-BMG:2009
44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44 44
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Seamless Tube Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Fittings Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Rod & Bar Rod & Bar Rod & Bar Rod & Bar Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless Pipe & Tube
42Fe-30Ni-21.5Cr-3Mo-2.3Cu 36Fe-35Ni-20Cr-4Cu-2Mo 31Ni-31Fe-27Cr-7Mo 37Ni-28Fe-25Cr-3Co-2Mo-2W 43Fe-35.5Ni-18.5Cr-Si 46Fe-24Ni-21Cr-6.5Mo-N 44Fe-33Ni-21Cr 44Fe-32.5Ni-21Cr-Al-Ti 42Fe-33Ni-21Cr-Al-Ti 42Fe-22MinNi-21.5Cr-3Mo-2Cu 44Fe-25.5Ni-21Cr-4.5Mo-1.5Cu 46Fe-25Ni-20Cr-6.5Mo-1Cu-N 45Fe-25Ni-20Cr-6.5Mo-1Cu-Mn-N 33Fe-33Cr-31.5Ni-1Mo-1Mn-Cu-N 30Fe-22Cr-21Ni-18.5Co-3Mo-2.7W 37Ni-28Fe-25Cr-3Co-2Mo-2W 42Fe-33Ni-21Cr 45Fe-32Ni-20.5Cr 47Fe-32Ni-20.5Cr 39.5Fe-32.5Ni-21Cr-1Mn-Cb 37Ni-28Fe-25Cr-3Co-2Mo-2W 42Fe-33Ni-21Cr 47Fe-32Ni-20.5Cr 39.5Fe-32.5Ni-21Cr-1Mn-Cb 37Ni-28Fe-25Cr-3Co-2Mo-2W 42Fe-33Ni-21Cr 47Fe-32Ni-20.5Cr 39.5Fe-32.5Ni-21Cr-1Mn-Cb 41Ni-30Fe-21Cr-5.7Mo-2Cu
Nickel and Nickel Base Alloys
164
45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 163 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 366 B 407 B 407 B 407 B 407 B 407 B 408 B 408 B 408 B 408 B 409 B 409 B 409 B 409 B 423
Ni-Fe-Cr (Alloy 825) CR20CB/WP20CB CR3127/WP3127 CRH120/WPH120 CR330/WP330 CR6XN/WP6XN CRNIC/WPNIC CRNIC10/WPNIC10 CRNIC11/WPNIC11 CRNICMC/WPNICMC CR904L/WP904L CR1925/WP1925 CR1925N/WP1925N CR3033/WP3033 CRH556/WPH556 Alloy HR120 Alloy 800 Alloy 801 Alloy 800H Alloy 800 HT Alloy HR120 Alloy 800 Alloy 800H Alloy 800HT Alloy HR120 Alloy 800 Alloy 810 Alloy 811 Alloy 20Cb3Mod.
N08825 N08020 N08031 N08120 N08330 N08367 N08800 N08810 N08811 N08825 N08904 N08925 N08926 R20033 R30556 N08120 N08800 N08801 N08810 N08811 N08120 N08800 N08810 N08811 N08120 N08800 N08810 N08811 N08221
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
85/35 [586/241] 80/35 [552/241] 94/40 [648/276] 90/40 [621/276] 70/30 [483/207] 95/45 [655/310] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 85/35 [586/241] 71/31 [490/214] 87/– [600/–] 87/– [600/–] 109/55 [752/379] 100/45 [689/310] 90/40 [621/276] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 65/25 [448/172] 90/40 [621/276] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 90/40 [621/276] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 79/34 [545/234] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Nickel and Nickel Base Alloys
165
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 423 B 424 B 424 B 425 B 425 B 435 B 462
Alloy 825 Alloy 20Cb3Mod. Alloy 825 Alloy 20Cb3Mod. Alloy 825 Alloy 556 Alloy 20Cb3
N08825 N08221 N08825 N08221 N08825 R30556 N08020
— — — — — — —
75/25 [517/172] 79/34 [545/234] 85/35 [586/241] 79/34 [545/234] 85/35 [586/241] 100/45 [689/310] 80/35 [552/241]
45
ASTM
B 462
Alloy 20Mo-4
N08024
—
80/35 [552/241]
45
ASTM
B 462
Alloy 20 Mo-6
N08026
—
80/35 [552/241]
45
ASTM
B 462
Alloy 6XN
N08367
—
95/45 [655/310]
45
ASTM
B 462
Alloy 33
R20033
—
109/55 [752/379]
45 45 45 45 45 45 45 45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 463 B 463 B 463 B 464 B 464 B 464 B 468 B 468 B 468 B 473 B 473 B 473 B 511 B 511
Alloy 20Cb3 Alloy 20Mo-4 Alloy 20 Mo-6 Alloy 20Cb3 Alloy 20Mo-4 Alloy 20 Mo-6 Alloy 20Cb3 Alloy 20Mo-4 Alloy 20 Mo-6 Alloy 20Cb3 Alloy 20Mo-4 Alloy 20 Mo-6 Alloy 330 Alloy 330 TX
N08020 N08024 N08026 N08020 N08024 N08026 N08020 N08024 N08026 N08020 N08024 N08026 N08330 N08332
— — — — — — — — — — — — — —
80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 80/35 [552/241] 70/30 [483/207] 67/27 [462/186] (Continued)
Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Rod & Bar Rod & Bar Plate, Sheet & Strip Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Forged or Rolled Pipe Flanges, etc. Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Bars Bars Bars Bars & Shapes Bars & Shapes
42Ni-30Fe-21.5Cr-3Mo-2.3Cu 41Ni-30Fe-21Cr-5.7Mo-2Cu 42Ni-30Fe-21.5Cr-3Mo-2.3Cu 41Ni-30Fe-21Cr-5.7Mo-2Cu 42Ni-30Fe-21.5Cr-3Mo-2.3Cu 30Fe-22Cr-21Ni-18Co-3Mo-2.7W 35Ni-35Fe-20Cr-3Cb-2.5Mo 37Ni-33Fe-24Cr-4Mo-2Cu 35Ni-31Fe-24Cr-6Mo-3Cu 46Fe-24Ni-21Cr-6.5Mo-Cu-N 33Fe-33Cr-32Ni-Mo-Cu-N 35Ni-35Fe-20Cr-3Cb-2.5Mo 37Ni-33Fe-24Cr-4Mo-2Cu 35Ni-31Fe-24Cr-6Mo-3Cu 35Ni-35Fe-20Cr-3Cb-2.5Mo 37Ni-33Fe-24Cr-4Mo-2Cu 35Ni-31Fe-24Cr-6Mo-3Cu 35Ni-35Fe-20Cr-3Cb-2.5Mo 37Ni-33Fe-24Cr-4Mo-2Cu 35Ni-31Fe-24Cr-6Mo-3Cu 35Ni-35Fe-20Cr-3Cb-2.5Mo 37Ni-33Fe-24Cr-4Mo-2Cu 35Ni-31Fe-24Cr-6Mo-3Cu 43Fe-35.5Ni-18.5Cr-Si 42Fe-35.5Ni-18.5Cr-1Si-Ti
AWS B2.1/B2.1M-BMG:2009
45 45 45 45 45 45 45
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Nickel and Nickel Base Alloys
166
45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 512 B 514 B 514 B 514 B 515 B 515 B 515 B 515 B 535 B 535 B 536 B 536 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 564 B 572
45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 599 B 619 B 619 B 619 B 619 B 620 B 621
Alloy 330 Alloy HR120 Alloy 800 Alloy 800H Alloy HR120 Alloy 800 Alloy 800H Alloy 800HT Alloy 330 Alloy 330TX Alloy 330 Alloy 330TX Alloy 31 Alloy HR120 Alloy AL-6XN Alloy 800 Alloy 800H Alloy 800HT Alloy 825 Alloy 33 Fe-Cr-Ni-Co-Mo-W (Alloy 556) Alloy 700 Alloy 31 Alloy 20 Mod. Alloy 33 Alloy 556 Alloy 20 Mod. Alloy 20 Mod.
N08330 N08120 N08800 N08810 N08120 N08800 N08810 N08811 N08330 N08332 N08330 N08332 N08031 N08120 N08367 N08800 N08810 N08811 N08825 R20033 R30556
— — — — — — — — — — — — — — — — — — — — —
70/30 [483/207] 90/40 [621/276] 75/30 [517/207] 65/25 [448/172] 90/40 [621/276] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 70/30 [483/207] 67/27 [462/186] 70/30 [483/207] 67/27 [462/186] 94/40 [648/276] 90/40 [621/276] 95/45 [655/310] 75/30 [517/207] 65/25 [448/172] 65/25 [448/172] 85/35 [586/241] 109/55 [752/379] 100/45 [689/310]
Billets & Bars Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Welded Tube Welded Tube Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Rod
43Fe-35.5Ni-18.5Cr-1Si 37Ni-30Fe-25Cr-Co-Mo-Cb 44Fe-33Ni-21Cr 44Fe-33Ni-21Cr 37Ni-30Fe-25Cr-Co-Mo-Cb 44Fe-33Ni-21Cr 44Fe-33Ni-21Cr 42Fe-33Ni-21Cr-Al-Ti 43Fe-35.5Ni-18.5Cr-Si 42Fe-35.5Ni-18.5Cr-1Si-Ti 43Fe-35.5Ni-18.5Cr-Si 42Fe-35.5Ni-18.5Cr-1Si-Ti 31Ni-31Fe-27Cr-7Mo-Cu 37Ni-30Fe-25Cr-Mo-Cb 46Fe-24Ni-21Cr-6.5Mo 44Fe-33Ni-21Cr 44Fe-33Ni-21Cr 42Fe-33Ni-21Cr-Al-Ti 42Ni-30Fe-21.5Cr-3Mo-2.3Cu 33Fe-33Cr-32Ni-Mo-Cu-N 33Fe-22Cr-21Ni-18Co-3Mo-3W
N08700 N08031 N08320 R20033 R30556 N08320 N08320
— — — — — — —
80/35 [552/241] 94/40 [648/276] 75/28 [517/193] 109/55 [752/379] 100/45 [689/310] 75/28 [517/193] 75/28 [517/193]
Plate, Sheet & Strip Welded Pipe Welded Pipe Welded Pipe Welded Pipe Plate, Sheet & Strip Rod
47Fe-25Ni-21Cr-5Mo 31Fe-31Ni-27Cr-7Mo-Cu 43Fe-26Ni-22Cr-5Mo 33Fe-33Cr-32Ni-Mo-Cu-N 30Fe-22Cr-21Ni-18Co-3Mo-2.7W 43Fe-26Ni-22Cr-5Mo 43Fe-26Ni-22Cr-5Mo
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Welded Tube Welded Tube Welded Tube Welded Tube Bar & Wire Bar & Wire Bar & Wire Bar & Wire Bar & Wire Seamless Tube Bar Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube
31Fe-31Ni-27Cr-7Mo-Cu 36Ni-35Fe-22Cr-4.5Mo 43Fe-26Ni-22Cr-5Mo 37Fe-33Ni-25.5Cr-3.2Mo-Cu 33Fe-33Cr-32Ni-Mo-Cu-N 30Fe-22Cr-21Ni-18Co-3Mo-2.7W 31Fe-31Ni-27Cr-7Mo-Cu 44Fe-25Ni-21Cr-4.5Mo 44Fe-25Ni-20Cr-6.5Mo-Cu-N 44Fe-25Ni-20Cr-6.5Mo-Cu-N 41Fe-25Ni-25Cr-5.5Mo-Cu-N 33Fe-33Cr-32Ni-Mo-Cu-N 33Fe-33Cr-32Ni-Mo-Cu-N 30Fe-22Cr-21Ni-18Co-3Mo-2.7W 31Fe-31Ni-27Cr-7Mo-Cu 43Fe-26Ni-22Cr-5Mo 31Fe-31Ni-27Cr-7Mo-Cu 44Fe-25Ni-21Cr-4.5Mo 44Fe-25Ni-20Cr-6Mo-Cu-N 44Fe-25Ni-20Cr-6.5Mo-Cu-N 33Fe-33Cr-31.5Ni-Mo-Cu-N 31Ni-31Fe-29Cr-Mo 47Fe-25Ni-21Cr-5Mo-Cb 44Fe-25Ni-21Cr-4.5Mo-Cu 46Fe-25Ni-20Cr-6Mo-Cu-N 35Ni-31Fe-24Cr-6Mo-3Cu 44Fe-25Ni-21Cr-4.5Mo-Cu 46Fe-25Ni-20Cr-6Mo-Cu-N 35Ni-31Fe-24Cr-6Mo-3Cu
Nickel and Nickel Base Alloys
167
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 622 B 622 B 622 B 622 B 622 B 622 B 625 B 625 B 625 B 625 B 625 B 625 B 626 B 626 B 626 B 626 B 649 B 649 B 649 B 649 B 649 B 668 B 672 B 673 B 673 B 673 B 674 B 674 B 674
Alloy 31 Alloy 2035 Alloy 20 Mod. Fe -Ni-Cr- Mo-Cu Alloy 33 Alloy 556 Alloy 31 Alloy 904L Alloy 1925 Alloy 926 Alloy UR-SB-8 Alloy 33 Alloy 33 Alloy 556 Alloy 31 Alloy 20 Mod. Alloy 31 Alloy 904L Alloy 1925 Alloy 926 Alloy 33 Alloy 28 Alloy 700 Alloy 904L Alloy 1925 Alloy 926 Alloy 904L Alloy 1925 Alloy 926
N08031 N08135 N08320 N08535 R20033 R30556 N08031 N08904 N08925 N08926 N08932 R20033 R20033 R30556 N08031 N08320 N08031 N08904 N08925 N08926 R20033 N08028 N08700 N08904 N08925 N08926 N08904 N08925 N08926
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
94/40 [648/276] 73/31 [503/214] 75/28 [517/193] 73/31 [503/214] 109/55 [752/379] 100/45 [689/310] 94/40 [648/276] 71/31 [490/214] 87/43 [600/296] 94/43 [648/296] 87/44 [600/303] 109/55 [752/379] 109/55 [752/379] 100/45 [689/310] 94/40 [648/276] 75/28 [517/193] 94/40 [648/276] 71/31 [490/214] 87/43 [600/296] 94/43 [648/296] 109/55 [752/379] 73/31 [503/214] 80/35 [552/241] 71/31 [490/214] 87/43 [600/296] 94/43 [648/296] 71/31 [490/214] 87/43 [600/296] 94/43 [648/296] (Continued)
AWS B2.1/B2.1M-BMG:2009
45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45 45
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
— 100/45 [689/310] 95/45 [655/310] 100/45 [689/310] 95/45 [655/310] 71/31 [490/214] 87/43 [600/296] 94/43 [648/296] — 100/45 [689/310] 95/45 [655/310]
Welded Pipe Welded Pipe Welded Pipe Welded Tube Welded Tube Seamless Pipe & Tube Seamless Pipe & Tube Seamless Pipe & Tube Sheet & Strip Sheet & Strip Plate
— 46Fe-24Ni-21Cr-6Mo-Cu-N 46Fe-24Ni-21Cr-6Mo-Cu-N 46Fe-24Ni-21Cr-6Mo-Cu-N 46Fe-24Ni-21Cr-6Mo-Cu-N 44Fe-25Ni-21Cr-4.5Mo-Cu 46Fe-25Ni-20Cr-6Mo-Cu-N 35Ni-31Fe-24Cr-6Mo-3Cu — 46Fe-24Ni-21Cr-6Mo-Cu-N 46Fe-24Ni-21Cr-6Mo-Cu-N
— 100/45 [689/310] 95/45 [655/310]
Sheet & Strip Seamless Pipe & Tube Seamless Pipe & Tube
— 46Fe-24Ni-21Cr-6Mo-Cu-N 46Fe-24Ni-21Cr-6Mo-Cu-N
Nickel and Nickel Base Alloys
168
45 45 45 45 45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 675 B 675 B 675 B 676 B 676 B 677 B 677 B 677 B 688 B 688 B 688
Fe-Ni-Cr-Mo Alloy AL-6XN Alloy AL-6XN Alloy AL-6XN Alloy AL-6XN Alloy 904L Alloy 1925 Alloy 926 Fe-Ni-Cr-Mo Alloy AL-6XN Alloy AL-6XN
N08366 N08367 N08367 N08367 N08367 N08904 N08925 N08926 N08366 N08367 N08367
45 45 45
ASTM ASTM ASTM
B 690 B 690 B 690
Fe-Ni-Cr-Mo Alloy AL-6XN Alloy AL-6XN
N08366 N08367 N08367
45 45 45 45 45 45 45 45 45 45 45 45 45
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 691 B 691 B 704 B 705 B 709 B 710 B 710 B 718 B 719 B 720 B 722 B 723 B 726
Fe-Ni-Cr-Mo Alloy AL-6XN Alloy 825 Alloy 825 Alloy 28 Alloy 330 Alloy 330TX Alloy 333 Alloy 333 Fe-Cr-Ni-Mo Alloy 333 Alloy 333 Alloy 333
N08366 N08367 N08825 N08825 N08028 N08330 N08332 N06333 N06333 N08310 N06333 N06333 N06333
— ≤3/16 [5] >3/16 [5] ≤3/16 [5] >3/16 [5] — — — — ≤3/16 [5] >3/16 ≤3/4 [>5 ≤19] — ≤3/16 [5] >3/16 ≤3/4 [>5 ≤19] — — — — — — — — — — — — —
— Round & Square Rods & Bars — 95/45 [655/310] Round & Sq. Rods & Bars 46Fe-24Ni-21Cr-6Mo-Cu-N 85/35 [586/241] Welded Tube 42Ni-30Fe-21.5Cr-3Mo-2.3Cu 85/35 [586/241] Welded Pipe 42Ni-30Fe-21.5Cr-3Mo-2.3Cu 73/31 [503/214] Plate, Sheet & Strip 31Ni-31Fe-29Cr-Mo 70/30 [483/207] Welded Pipe 42Fe-35.5Ni-18.5Cr-Si 67/27 [462/186] Welded Pipe 42Fe-35.5Ni-18.5Cr-Si 80/35 [552/241] Plate, Sheet & Strip 46Ni-25.5Cr-16Fe-3.3Mo-3.3W-3.3Co 80/35 [552/241] Bars 46Ni-25.5Cr-16Fe-3.3Mo-3.3W-3.3Co — Seamless Tube — 80/35 [552/241] Seamless Pipe & Tube 46Ni-25.5Cr-16Fe-3.3Mo-3.3W-3.3Co 80/35 [552/241] Welded Pipe 46Ni-25.5Cr-16Fe-3.3Mo-3.3W-3.3Co 80/35 [552/241] Welded Tube 46Ni-25.5Cr-16Fe-3.3Mo-3.3W-3.3Co
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number List of Base Metals—Nonferrous Alloys
Material Base Metal Number Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Welded Pipe & Tube Welded Pipe & Tube Seamless Tube Rod & Bar Seamless Pipe & Tube Plate, Sheet & Strip Fittings Fittings Plate, Sheet & Strip Welded Tube Welded Pipe Forging Forging Rod Welded Pipe Seamless Pipe & Tube Welded Tube
46Fe-24Ni-21Cr-6.5Mo-Cu-W 46Fe-24Ni-21Cr-6.5Mo-Cu-W 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 37Ni-30Co-28Cr-2.7Si-Ti 37Ni-30Co-28Cr-2.7Si-Ti 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 46Ni-27.5Cr-23Fe-2.75Si 37Ni-30Co-28Cr-2.7Si-Ti 37Ni-30Co-28Cr-2.7Si-Ti 37Ni-30Co-28Cr-2.7Si-Ti 37Ni-30Co-28Cr-2.7Si-Ti 37Ni-30Co-28Cr-2.7Si-Ti
Nickel and Nickel Base Alloys
169
45 45 46 46 46 46 46 46 46 46 46 46 46 46 46 46 46
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 804 B 804 B 163 B 166 B 167 B 168 B 366 B 366 B 435 B 516 B 517 B 564 B 564 B 572 B 619 B 622 B 626
Alloy AL-6XN Alloy AL-6XN Ni-Cr-Fe-Si (Alloy 45) Ni-Cr-Fe (Alloy 45) Ni-Cr-Fe (Alloy 45) Alloy 45 CRV45TM/WPV45TM CRH160/WPH160 Alloy HR160 Alloy 45 Alloy 45 Alloy 45 Alloy HR160 Alloy HR160 Alloy HR160 Alloy HR160 Alloy HR160
N08367 N08367 N06045 N06045 N06045 N06045 N06045 N12160 N12160 N06045 N06045 N06045 N12160 N12160 N12160 N12160 N12160
≤3/16 [5] >3/16 [5] — — — — — — — — — — — — — — —
100/45 [689/310] 95/45 [655/310] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241] 90/35 [621/241]
AWS B2.1/B2.1M-BMG:2009
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished)
UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd 0.11Ru 0.11Ru 0.5Co-0.06Ru 0.45Ni-0.15Cr-Ru-Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd 0.11Ru 0.5Co-0.06Pd 0.45Ni-0.15Cr-Ru-Pd UnalloyedTi UnalloyedTi UnalloyedTi
Titanium and Titanium Base Alloys
170
51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 337 B 337 B 337 B 337 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 338 B 348 B 348 B 348
Grade 1 Grade 2 Grade 7 Grade 11 Grade 13 Grade 16 Grade 17 Grade 26 Grade 27 Grade 30 Grade 33 Grade 1 Grade 2 Grade 7 Grade 11 Grade 1 Grade 2 Grade 7 Grade 11 Grade 13 Grade 16 Grade 17 Grade 27 Grade 30 Grade 33 Grade 1 Grade 1 Grade 1
R50250 R50400 R52400 R52250 R53413 R52402 R52252 — — — — R50250 R50400 R52400 R52250 R50250 R50400 R52400 R52250 R53413 R52402 R52252 — — — R50250 R50250 R50250
— — — — — — — — — — — — — — — — — — — — — — — — — — — —
35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished)
UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.06Pd 0.06Pd 0.06Pd 0.06Pd 0.06Pd 0.06Pd 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.18Pd 0.06Pd 0.06Pd
Titanium and Titanium Base Alloys
171
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348
Grade 1 Grade 1 Grade 1 Grade 2 Grade 2 Grade 2 Grade 2 Grade 2 Grade 2 Grade 11 Grade 11 Grade 11 Grade 11 Grade 11 Grade 11 Grade 17 Grade 17 Grade 17 Grade 17 Grade 17 Grade 17 Grade 7 Grade 7 Grade 7 Grade 7 Grade 7 Grade 7 Grade 16 Grade 16
R50250 R50250 R50250 R50400 R50400 R50400 R50400 R50400 R50400 R52250 R52250 R52250 R52250 R52250 R52250 R52252 R52252 R52252 R52252 R52252 R52252 R52400 R52400 R52400 R52400 R52400 R52400 R52402 R52402
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] (Continued)
AWS B2.1/B2.1M-BMG:2009
51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings
0.06Pd 0.06Pd 0.06Pd 0.06Pd 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Co-0.06Pd 0.5Co-0.06Pd 0.5Co-0.06Pd 0.5Co-0.06Pd 0.5Co-0.06Pd 0.5Co-0.06Pd 0.45Ni-Cr-Ru-Pd 0.45Ni-Cr-Ru-Pd 0.45Ni-Cr-Ru-Pd 0.45Ni-Cr-Ru-Pd 0.45Ni-Cr-Ru-Pd 0.45Ni-Cr-Ru-Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd
Titanium and Titanium Base Alloys
172
51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 363 B 363 B 363 B 363 B 363 B 363 B 363
Grade 16 Grade 16 Grade 16 Grade 16 Grade 13 Grade 13 Grade 13 Grade 13 Grade 13 Grade 13 Grade 30 Grade 30 Grade 30 Grade 30 Grade 30 Grade 30 Grade 33 Grade 33 Grade 33 Grade 33 Grade 33 Grade 33 WPT 1 WPT 2 WPT 7 WPT 11 WPT 13 WPT 16 WPT 17
R52402 R52402 R52402 R52402 R53413 R53413 R53413 R53413 R53413 R53413 — — — — — — — — — — — — R50250 R50400 R52400 R52250 R53413 R52402 R52252
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 40/25 [276/172] 40/25 [276/172] 40/25 [276/172] 40/25 [276/172] 40/25 [276/172] 40/25 [276/172] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Seamless & Welded Fittings Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Castings (As-Cast) Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Forgings Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
0.5Ni-0.06Pd UnalloyedTi 0.06Pd 0.12minPd 0.06Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd 0.5Co-0.06Pd 0.4Ni-0.15Cr-Ru-Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd 0.4Ni-0.15Cr-Ru-Pd UnalloyedTi UnalloyedTi 0.18Pd 0.18Pd 0.5Ni-0.05Ru 0.06Pd 0.06Pd
Titanium and Titanium Base Alloys
173
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 363 B 367 B 367 B 367 B 367 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 381 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 861 B 862 B 862 B 862 B 862 B 862 B 862 B 862
WPT 30 Grade C-2 Pd 17 Pd 7B Pd 16 F-1 F-2 F-7 F-11 F-13 F-16 F-17 F-30 F-33 Grade 1 Grade 2 Grade 7 Grade 11 Grade 13 Grade 16 Grade 17 Grade 33 Grade 1 Grade 2 Grade 7 Grade 11 Grade 13 Grade 16 Grade 17
— R50400 R52252 R52401 R52402 R50250 R50400 R52400 R52250 R53413 R52402 R52252 — — R50250 R50400 R52400 R52250 R53413 R52402 R52252 — R50250 R50400 R52400 R50250 R53413 R52402 R52252
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 35/25 [241/172] 50/40 [345/276] 50/40 [345/276] 35/25 [241/172] 40/25 [276/172] 50/40 [345/276] 35/25 [241/172] (Continued)
AWS B2.1/B2.1M-BMG:2009
51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51 51
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Welded Pipe Welded Pipe Welded Pipe
0.11Ru 0.11Ru 0.4Ni-0.15Cr-Ru-Pd
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished)
UnalloyedTi 0.75Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Co-0.06Pd 0.4Ni-0.15Cr-Ru-Pd UnalloyedTi 0.75Ni-0.3Mo UnalloyedTi 0.75Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Co-0.06Pd 0.4Ni-0.15Cr-Ru-Pd UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi 0.75Ni-0.3Mo 0.75Ni-0.3Mo 0.75Ni-0.3Mo 0.75Ni-0.3Mo 0.75Ni-0.3Mo
Titanium and Titanium Base Alloys
174
51 51 51
ASTM ASTM ASTM
B 862 B 862 B 862
Grade 26 Grade 27 Grade 33
R52404 R52254 —
— — —
50/40 [345/276] 35/25 [241/172] 50/40 [345/276]
52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 265 B 265 B 265 B 265 B 265 B 265 B 337 B 337 B 338 B 338 B 338 B 338 B 338 B 338 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348
Grade 3 Grade 12 Grade 14 Grade 15 Grade 31 Grade 34 Grade 3 Grade 12 Grade 3 Grade 12 Grade 14 Grade 15 Grade 31 Grade 34 Grade 3 Grade 3 Grade 3 Grade 3 Grade 3 Grade 3 Grade 12 Grade 12 Grade 12 Grade 12 Grade 12
R50550 R53400 R53414 R53415 — — R50550 R53400 R50550 R53400 R53414 R53415 — — R50550 R50550 R50550 R50550 R50550 R50550 R53400 R53400 R53400 R53400 R53400
— — — — — — — — — — — — — — — — — — — — — — — — —
65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 70/55 [483/379] 65/55 [448/379] 65/55 [448/379] 66/55 [455/379] 70/50 [483/345] 65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 70/55 [483/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 70/50 [483/345] 70/50 [483/345] 70/50 [483/345] 70/50 [483/345] 70/50 [483/345] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings
0.75Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.3Co-0.05Pd 0.3Co-0.05Pd 0.3Co-0.05Pd 0.3Co-0.05Pd 0.3Co-0.05Pd 0.3Co-0.05Pd 0.4Ni-Cr-Ru-Pd 0.4Ni-Cr-Ru-Pd 0.4Ni-Cr-Ru-Pd 0.4Ni-Cr-Ru-Pd 0.4Ni-Cr-Ru-Pd 0.4Ni-Cr-Ru-Pd UnalloyedTi 0.75Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru
Titanium and Titanium Base Alloys
175
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 363 B 363 B 363 B 363
Grade 12 Grade 14 Grade 14 Grade 14 Grade 14 Grade 14 Grade 14 Grade 15 Grade 15 Grade 15 Grade 15 Grade 15 Grade 15 Grade 31 Grade 31 Grade 31 Grade 31 Grade 31 Grade 31 Grade 34 Grade 34 Grade 34 Grade 34 Grade 34 Grade 34 WPT 3 WPT 12 WPT 14 WPT 15
R53400 R53414 R53414 R53414 R53414 R53414 R53414 R53415 R53415 R53415 R53415 R53415 R53415 — — — — — — — — — — — — R50550 R53400 R53414 R53415
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
70/50 [483/345] 60/40 [414/276] 60/40 [414/276] 60/40 [414/276] 60/40 [414/276] 60/40 [414/276] 60/40 [414/276] 70/55 [483/379] 70/55 [483/379] 70/55 [483/379] 70/55 [483/379] 70/55 [483/379] 70/55 [483/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 65/55 [448/379] (Continued)
AWS B2.1/B2.1M-BMG:2009
52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Castings (As-Cast) Castings (As-Cast) Forgings Forgings Forgings Forgings Forgings Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Welded Pipe
UnalloyedTi 0.12minPd UnalloyedTi 0.75Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.3Co-0.05Pd UnalloyedTi 0.8Ni-0.3Mo 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.4Ni-0.15Cr-Ru-Pd UnalloyedTi 0.03Co-0.05Pd 0.5Ni-0.05Ru 0.5Ni-0.05Ru 0.4Ni-0.15Cr-Ru-Pd
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Seamless & Welded Pipe Seamless & Welded Tube Seamless & Welded Tube
UnalloyedTi 3Al-2.5V 3Al-2.5V-0.06Pd 3Al-2.5V-0.11Ru 15Mo-3Al-2.7Nb-0.25Si 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 5Al-1Sn-1Zr-1V-0.9Mo 3Al-2.5V 3Al-2.5V 3Al-2.5V-0.06Pd
Titanium and Titanium Base Alloys
176
52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52 52
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 367 B 367 B 381 B 381 B 381 B 381 B 381 B 861 B 861 B 861 B 861 B 861 B 862 B 862 B 862 B 862 B 862
Grade C-3 Pd 8A F-3 F-12 F-14 F-15 F-31 Grade 3 Grade 12 Grade 14 Grade 15 Grade 34 Grade 3 Grade 12 Grade 14 Grade 15 Grade 34
R50550 R52401 R50550 R53400 R53414 R53415 — R50550 R53400 R53414 R53415 — R50550 R53400 R53414 R53415 —
— — — — — — — — — — — — — — — — —
53 53 53 53 53 53 53 53 53 53 53
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 265 B 337 B 338 B 338
Grade 4 Grade 9 Grade 18 Grade 28 Grade 21 Grade 19 Grade 20 Grade 32 Grade 9 Grade 9 Grade 18
R50700 R56320 R56322 R56323 R58210 R58640 R58645 — R56320 R56320 R56322
— — — — — — — — — — —
65/55 [448/379] 65/55 [448/379] 65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 70/55 [483/379] 65/55 [448/379] 65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 70/55 [483/379] 65/55 [448/379] 65/55 [448/379] 70/50 [483/345] 60/40 [414/276] 70/55 [483/379] 65/55 [448/379] 80/70 [552/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 115/110 [793/758] 115/110 [793/758] 115/110 [793/758] 100/85 [689/586] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Titanium and Titanium Base Alloys
177
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 338 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348
Grade 28 Grade 4 Grade 4 Grade 4 Grade 4 Grade 4 Grade 4 Grade 9 Grade 9 Grade 9 Grade 9 Grade 9 Grade 9 Grade 18 Grade 18 Grade 18 Grade 18 Grade 18 Grade 18 Grade 21
R56323 R50700 R50700 R50700 R50700 R50700 R50700 R56320 R56320 R56320 R56320 R56320 R56320 R56322 R56322 R56322 R56322 R56322 R56322 R58210
— — — — — — — — — — — — — — — — — — — —
90/70 [621/483] 80/70 [552/483] 80/70 [552/483] 80/70 [552/483] 80/70 [552/483] 80/70 [552/483] 80/70 [552/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 115/110 [793/758]
53
ASTM
B 348
Grade 21
R58210
—
115/110 [793/758]
53 53 53
ASTM ASTM ASTM
B 348 B 348 B 348
Grade 21 Grade 21 Grade 21
R58210 R58210 R58210
— — —
115/110 [793/758] 115/110 [793/758] 115/110 [793/758]
53
ASTM
B 348
Grade 21
R58210
—
115/110 [793/758]
(Continued)
Seamless & Welded Tube Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled) Hexagons & Octagons (Hot Rolled) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Rounds & Squares (Hot Rolled, Solution Treated) Hex. & Oct. (Hot Rolled, Solution Treated) Flat Bars (Hot Rolled, Solution Treated) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished, Solution Treated) Flat Bars (Cold Finished, (Cold Finished, Solution Treated)
3Al-2.5V-0.11Ru UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi UnalloyedTi 3Al-2.5V 3Al-2.5V 3Al-2.5V 3Al-2.5V 3Al-2.5V 3Al-2.5V 3Al-2.5V-0.06Pd 3Al-2.5V-0.06Pd 3Al-2.5V-0.06Pd 3Al-2.5V-0.06Pd 3Al-2.5V-0.06Pd 3Al-2.5V-0.06Pd 15Mo-3Al-2.7Nb-0.25Si 15Mo-3Al-2.7Nb-0.25Si 15Mo-3Al-2.7Nb-0.25Si 15Mo-3Al-2.7Nb-0.25Si 15Mo-3Al-2.7Nb-0.25Si 15Mo-3Al-2.7Nb-0.25Si
AWS B2.1/B2.1M-BMG:2009
53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Titanium and Titanium Base Alloys
178
53
ASTM
B 348
Grade 19
R58640
—
115/110 [793/758]
53
ASTM
B 348
Grade 19
R58640
—
115/110 [793/758]
53 53 53
ASTM ASTM ASTM
B 348 B 348 B 348
Grade 19 Grade 19 Grade 19
R58640 R58640 R58640
— — —
115/110 [793/758] 115/110 [793/758] 115/110 [793/758]
53
ASTM
B 348
Grade 19
R58640
—
115/110 [793/758]
53
ASTM
B 348
Grade 20
R58645
—
115/110 [793/758]
53
ASTM
B 348
Grade 20
R58645
—
115/110 [793/758]
53 53
ASTM ASTM
B 348 B 348
Grade 20 Grade 20
R58645 R58645
— —
115/110 [793/758] 115/110 [793/758]
53
ASTM
B 348
Grade 20
R58645
—
115/110 [793/758]
53
ASTM
B 348
Grade 20
R58645
—
115/110 [793/758]
53
ASTM
B 348
Grade 32
—
—
100/85 [689/586]
53
ASTM
B 348
Grade 32
—
—
100/85 [689/586]
53 53 53
ASTM ASTM ASTM
B 348 B 348 B 348
Grade 32 Grade 32 Grade 32
— — —
— — —
100/85 [689/586] 100/85 [689/586] 100/85 [689/586]
53
ASTM
B 348
Grade 32
—
—
100/85 [689/586]
53
ASTM
B 363
WPT 9
R56320
—
90/70 [621/483] (Continued)
Rounds & Squares (Hot Rolled, (Cold Finished, Solution Treated) Hex. & Oct. (Hot Rolled, Solution Treated) Flat Bars (Hot Rolled, Solution Treated) Rounds (Cold Finished, Solution Treated) Hex., Oct. & Squares (Cold Finished, Solution Treated) Flat Bars (Cold Finished, Solution Treated) Rounds & Squares (Hot Rolled, Solution Treated) Hex. & Oct. (Hot Rolled, Solution Treated) Flat Bars (Hot Rolled, Solution Treated) Rounds (Cold Finished, Solution Treated) Hex., Oct. & Squares (Cold Finished, Solution Treated) Flat Bars (Cold Finished, Solution Treated) Rounds & Squares (Hot Rolled, Solution Treated) Hex. & Oct. (Hot Rolled, Solution Treated) Flat Bars (Hot Rolled, Solution Treated) Rounds (Cold Finished, Solution Treated) Hex., Oct. & Squares (Cold Finished, Solution Treated) Flat Bars (Cold Finished, Solution Treated) Seamless & Welded Fittings
8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 5Al-1Sn-1Zr-1V-0.9Mo 5Al-1Sn-1Zr-1V-0.9Mo 5Al-1Sn-1Zr-1V-0.9Mo 5Al-1Sn-1Zr-1V-0.9Mo 5Al-1Sn-1Zr-1V-0.9Mo 5Al-1Sn-1Zr-1V-0.9Mo 3Al-2.5V
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Forgings Forgings Forgings Forgings (Solution Treated) Forgings (Solution Treated) Forgings (Solution Treated) Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe Sheet (Solution Treated)
3Al-2.5V-0.06Pd 15Mo-3Al-2.7Nb-0.25Si 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd UnalloyedTi 3Al-2.5V 3Al-2.5V-0.06Pd 15Mo-3Al-2.7Nb-0.25Si 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 3Al-2.5V 3Al-2.5V-0.06Pd 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 15Mo-3Al-2.7Nb-0.25Si 3Al-2.5V-0.11Ru 3Al-2.5V 3Al-2.5V-0.06Pd 8V-6Cr-4Zr-4Mo-3Al 8V-6Cr-4Zr-4Mo-3Al-0.06Pd 15Mo-3Al-2.7Nb-0.25Si 3Al-2.5V-0.11Ru 15V-3Cr-3Sn-3Al
Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip Plate, Sheet & Strip
6Al-4V 5Al-2.5Sn 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.11Ru
Titanium and Titanium Base Alloys
179
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM AMS
B 363 B 363 B 363 B 363 B 381 B 381 B 381 B 381 B 381 B 381 B 861 B 861 B 861 B 861 B 861 B 861 B 862 B 862 B 862 B 862 B 862 B 862 4914
WPT 18 WPT 21 WPT 19 WPT 20 F-4 F-9 F-18 F-21 F-19 F-20 Grade 9 Grade 18 Grade 19 Grade 20 Grade 21 Grade 28 Grade 9 Grade 18 Grade 19 Grade 20 Grade 21 Grade 28 15-3
R56322 R58210 R58640 R58645 R50700 R56320 R56322 R58210 R58640 R58645 R56320 R56322 R58640 R58645 R58210 R56323 R56320 R56322 R58640 R58645 R58210 R56323 R58153
— — — — — — — — — — — — — — — — — — — — — — —
90/70 [621/483] 115/110 [793/758] 115/110 [793/758] 115/110 [793/758] 80/70 [552/483] 90/70 [621/483] 90/70 [621/483] 115/110 [793/758] 115/110 [793/758] 115/110 [793/758] 90/70 [621/483] 90/70 [621/483] 115/110 [793/758] 115/110 [793/758] 140/130 [965/896] 90/70 [621/483] 90/70 [621/483] 90/70 [621/483] 115/110 [793/758] 115/110 [793/758] 140/130 [965/896] 90/70 [621/483] 98/96 [676/662]
54 54 54 54 54
ASTM ASTM ASTM ASTM ASTM
B 265 B 265 B 265 B 265 B 265
Grade 5 Grade 6 Grade 24 Grade 25 Grade 29
R56400 R54520 R56405 R56403 R56404
— — — — —
130/120 [896/827] 120/115 [827/724] 130/120 [896/827] 130/120 [896/827] 120/110 [827/758] (Continued)
AWS B2.1/B2.1M-BMG:2009
53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53 53
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Plate, Sheet & Strip Seamless & Welded Tube Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished)
4.5Al-2Mo-1.6V-Si-Fe 4.5Al-2Mo-1.6V-Si-Fe 6Al-4V 6Al-4V 6Al-4V 6Al-4V 6Al-4V 6Al-4V 5Al-2.5Sn 5Al-2.5Sn 5Al-2.5Sn 5Al-2.5Sn 5Al-2.5Sn 5Al-2.5Sn 6Al-4V(ELI) 6Al-4V(ELI) 6Al-4V(ELI) 6Al-4V(ELI) 6Al-4V(ELI) 6Al-4V(ELI) 6Al-4V-0.06Pd 6Al-4V-0.06Pd 6Al-4V-0.06Pd 6Al-4V-0.06Pd 6Al-4V-0.06Pd 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.55Ni-0.06Pd
Titanium and Titanium Base Alloys
180
54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 265 B 338 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348
Grade 35 Grade 35 Grade 5 Grade 5 Grade 5 Grade 5 Grade 5 Grade 5 Grade 6 Grade 6 Grade 6 Grade 6 Grade 6 Grade 6 Grade 23 Grade 23 Grade 23 Grade 23 Grade 23 Grade 23 Grade 24 Grade 24 Grade 24 Grade 24 Grade 24 Grade 24 Grade 25 Grade 25 Grade 25
— — R56400 R56400 R56400 R56400 R56400 R56400 R54520 R54520 R54520 R54520 R54520 R54520 R56402 R56402 R56402 R56402 R56402 R56402 R56405 R56405 R56405 R56405 R56405 R56405 R56403 R56403 R56403
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 120/115 [827/793] 120/115 [827/793] 120/115 [827/793] 120/115 [827/793] 120/115 [827/793] 120/115 [827/793] 120/110 [827/758] 120/110 [827/758] 120/110 [827/758] 120/110 [827/758] 120/110 [827/758] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] (Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Flat Bars (Cold Finished) Hex., Oct. & Squares (Cold Finished) Rounds (Cold Finished) Hexagons & Octagons (Hot Rolled) Rounds & Squares (Hot Rolled) Flat Bars (Hot Rolled) Seamless & Welded Fittings Seamless & Welded Fittings Seamless & Welded Fittings Castings (As-Cast) Castings (As-Cast) Forgings Forgings Forgings Forgings Forgings Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Seamless Pipe Welded Pipe Welded Pipe Welded Pipe Welded Pipe
6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.55Ni-0.06Pd 4Al-2Mo-1.6V-Fe-Si 4Al-2Mo-1.6V-Fe-Si 4Al-2Mo-1.6V-Fe-Si 4Al-2Mo-1.6V-Fe-Si 4Al-2Mo-1.6V-Fe-Si 4Al-2Mo-1.6V-Fe-Si 6Al-4V 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V 5Al-2.5Sn 6Al-4V 5Al-2.5Sn 6Al-4V 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V 6Al-4V(ELI) 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd 6Al-4V-0.11Pd(ELI) 4.5Al-2Mo-1.6V-0.5Fe-0.3Si 6Al-4V 6Al-4V(ELI) 6Al-4V-0.06Pd 6Al-4V-0.55Ni-0.06Pd
Titanium and Titanium Base Alloys
181
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 348 B 363 B 363 B 363 B 367 B 367 B 381 B 381 B 381 B 381 B 381 B 861 B 861 B 861 B 861 B 861 B 861 B 862 B 862 B 862 B 862
Grade 25 Grade 25 Grade 25 Grade 35 Grade 35 Grade 35 Grade 35 Grade 35 Grade 35 WPT 23 WPT 24 WPT 25 Grade C-5 Grade C-6 F-5 F-6 F-23 F-24 F-25 Grade 5 Grade 23 Grade 24 Grade 25 Grade 29 Grade 35 Grade 5 Grade 23 Grade 24 Grade 25
R56403 R56403 R56403 — — — — — — R56402 R56405 R56403 R56400 R54520 R56400 R54520 R56402 R56405 R56403 R56400 R56402 R56405 R56403 R56404 — R56400 R56402 R56405 R56403
— — — — — — — — — — — — — — — — — — — — — — — — — — — — —
130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 115/105 [793/724] 130/120 [896/827] 120/115 [827/793] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] 130/120 [896/827] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] 120/110 [827/758] 130/120 [896/827] 130/120 [896/827] (Continued)
AWS B2.1/B2.1M-BMG:2009
54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54 54
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Titanium and Titanium Base Alloys
182
54 54 54 54
ASTM ASTM AMS AMS
B 862 B 862 4915 4915
Grade 29 Grade 35 8Al-1Mo-1V 8Al-1Mo-1V
R56404 — R54810 R54810
54
AMS
4915
8Al-1Mo-1V
R54810
54
AMS
4915
8Al-1Mo-1V
R54810
54
AMS
4915
8Al-1Mo-1V
R54810
54 54 54
AMS AMS AMS
4919 4973 4973
Al-Zr-Mo-Sn Al-Mo-V Al-Mo-V
R54620 R54810 R54810
54 54
AMS AMS
4975 4976
Al-Zr-Mo-Sn Al-Zr-Mo-Sn
R54620 R54620
— 120/110 [827/758] Welded Pipe 6Al-4V-0.11Pd(ELI) — 130/120 [896/827] Welded Pipe 4.5Al-2Mo-1.6V-0.5Fe-0.3Si ≤0.187 [5] 145/135 [1000/931] Sheet & Strip (Single Annealed) 8Al-1Mo-1V 0.1875–0.500 145/135 [1000/931] Plate (Single Annealed) 8Al-1Mo-1V [5–13] 0.501–1.000 140/130 [965/896] Plate (Single Annealed) 8Al-1Mo-1V [13–25] 1.001–2.500 130/120 [896/827] Plate (Single Annealed) 8Al-1Mo-1V [25–64] 2.501–4.000 120/110 [827/758] Plate (Single Annealed) 8Al-1Mo-1V [64–100] — 135/125 [931/862] Sheet (Duplex Annealed) 6Al-4Zr-2Mo-2Sn ≤2.500 [64] 130/120 [896/827] Forgings (Solution Treated & Stabilized) 8Al-1Mo-1V 2.500–4.000 120/110 [827/758] Forgings (Solution Treated & Stabilized) 8Al-1Mo-1V [64–100] — 130/120 [896/827] Bar (Solution Treated, Duplex Annealed) 6Al-4Zr-2Mo-2Sn — 130/120 [896/827] Forging, STA (Duplex Annealed) 6Al-4Zr-2Mo-2Sn
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Zirconium and Zirconium Base Alloys
183
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 351 B 352 B 352 B 352 B 352 B 352 B 352 B 353 B 353 B 353 B 493 B 493
R60001 R60001 R60001 R60001 R60802 R60802 R60802 R60802 R60804 R60804 R60804 R60804 R60001 R60001 R60802 R60802 R60804 R60804 R60001 R60802 R60804 R60702 R60704
R60001 R60001 R60001 R60001 R60802 R60802 R60802 R60802 R60804 R60804 R60804 R60804 R60001 R60001 R60802 R60802 R60804 R60804 R60001 R60802 R60804 R60702 R60704
— — — — — — — — — — — — <3/16 [5] ≥3/16 [5] <3/16 [5] ≥3/16 [5] <3/16 [5] ≥3/16 [5] — — — — —
42/20 [290/138] 42/20 [290/138] 42/20 [290/138] 42/20 [290/138] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 60/35 [414/241] 42/20 [290/138] 42/20 [290/138] 58/35 [400/241] 58/35 [400/241] 56/35 [386/241] 58/35 [400/241] 42/20 [290/138] 60/35 [414/241] 60/35 [414/241] 55/30 [379/207] 60/35 [414/241]
Bars—Round, Square & Hexagon Flat Bars Rod Wire Bars—Round, Square & Hexagon Flat Bars Rod Wire Bars—Round, Square & Hexagon Flat Bars Rod Wire Sheet & Strip Plate Sheet & Strip Plate Sheet & Strip Plate Seamless & Welded Tube Seamless & Welded Tube Seamless & Welded Tube Forgings Forgings
61 61
ASTM ASTM
B 523 B 523
R60702 R60704
R60702 R60704
— —
55/30 [379/207] 60/35 [414/241]
Seamless & Welded Tube Seamless & Welded Tube
61 61
ASTM ASTM
B 550 B 550
R60702 R60702
R60702 R60702
— —
55/30 [379/207] 55/30 [379/207]
Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished)
(Continued)
99.9minZr 99.9minZr 99.9minZr 99.9minZr 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 99.9minZr 99.9minZr 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 99.9minZr 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) 99.2min(Zr+Hf) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 99.2min(Zr+Hf) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 99.2min(Zr+Hf) 99.2min(Zr+Hf)
AWS B2.1/B2.1M-BMG:2009
61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61 61
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Zirconium and Zirconium Base Alloys
184
61 61 61 61 61
ASTM ASTM ASTM ASTM ASTM
B 550 B 550 B 550 B 550 B 550
R60702 R60702 R60702 R60702 R60704
R60702 R60702 R60702 R60702 R60704
— — — — —
55/30 [379/207] 55/30 [379/207] 55/30 [379/207] 55/30 [379/207] 60/35 [414/241]
Flat Bars (Cold Finished) Round & Square Wire Flat Bars (Hot Rolled) Drawn Hexagons & Octagons Flat Bars (Hot Rolled)
61
ASTM
B 550
R60704
R60704
—
60/35 [414/241]
Rounds (Cold Finished)
61
ASTM
B 550
R60704
R60704
—
60/35 [414/241]
Hex., Oct. & Squares (Cold Finished)
61
ASTM
B 550
R60704
R60704
—
60/35 [414/241]
Flat Bars (Cold Finished)
61
ASTM
B 550
R60704
R60704
—
60/35 [414/241]
Round & Square Wire
61
ASTM
B 550
R60704
R60704
—
60/35 [414/241]
Drawn Hexagons & Octagons
61 61 61
ASTM ASTM ASTM
B 551 B 551 B 551
R60702 R60702 R60704
R60702 R60702 R60704
<3/16 [5] ≥3/16 [5] <3/16 [5]
55/30 [379/207] 55/30 [379/207] 60/35 [414/241]
Sheet & Strip Plate Sheet & Strip
61
ASTM
B 551
R60704
R60704
≥3/16 [5]
60/35 [414/241]
Plate
61 61
ASTM ASTM
B 658 B 658
R60702 R60704
R60702 R60704
— —
55/30 [379/207] 60/35 [414/241]
Seamless & Welded Pipe Seamless & Welded Pipe
62 62 62 62 62
ASTM ASTM ASTM ASTM ASTM
B 351 B 351 B 351 B 351 B 352
R60901 R60901 R60901 R60901 R60901
R60901 R60901 R60901 R60901 R60901
— 65/45 [448/310] — 65/45 [448/310] — 65/45 [448/310] — 65/45 [448/310] ≥3/16 [5] 65/45 [448/310] (Continued)
Bars—Round, Square & Hexagon Flat Bars Rod Wire Sheet & Strip
99.2min(Zr+Hf) 99.2min(Zr+Hf) 99.2min(Zr+Hf) 99.2min(Zr+Hf) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 99.2minZr 99.2minZr 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 99.2min(Zr+Hf) 97.5min(Zr+Hf)-1.5Sn0.3(Fe+Cr) 97.3Zr-2.6Cb 97.3Zr-2.6Cb 97.3Zr-2.6Cb 97.3Zr-2.6Cb 97.3Zr-2.6Cb
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Plate Seamless & Welded Tube Seamless & Welded Tube Forgings Seamless & Welded Tube Hex., Oct. & Squares (Cold Finished) Flat Bars (Hot Rolled) Rounds (Cold Finished) Hex., Oct. & Squares (Cold Finished) Flat Bars (Cold Finished) Round & Square Wire Drawn Hexagons & Octagons Plate, Sheet & Strip Plate, Sheet & Strip Seamless & Welded Pipe
97.3Zr-2.6Cb 97.3Zr-2.6Cb 97.35Zr-2.65Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb 95.5(Zr+Hf)-2.5Cb
Zirconium and Zirconium Base Alloys
185
62 62 62 62 62 62 62 62 62 62 62 62 62 62 62
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 352 B 353 B 353 B 493 B 523 B 550 B 550 B 550 B 550 B 550 B 550 B 550 B 551 B 551 B 658
R60901 R60901 R60904 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60706 R60705
R60901 R60901 R60904 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60705 R60706 R60705
>3/16 [5] — — — — — — — — — — — — — —
65/45 [448/310] 65/45 [448/310] 65/45 [448/310] 70/55 [483/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 80/55 [552/379] 74/50 [510/345] 80/55 [552/379]
AWS B2.1/B2.1M-BMG:2009
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
32/– [221/–]
Plate & Sheet
95.5Mg-3Al-1Zn
32/18 [221/124]
Sheet
95.5Mg-3Al-1Zn
32/15 [221/103]
Plate & Sheet
95.5Mg-3Al-1Zn
30/16 [207/110]
Plate & Sheet
95.5Mg-3Al-1Zn
30/15 [207/103]
Plate
95.5Mg-3Al-1Zn
29/14 [200/97]
Plate
95.5Mg-3Al-1Zn
30/18 [207/124]
Sheet
98Mg-1.25Zn-0.17Re
30/15 [207/103]
Sheet
98Mg-1.25Zn-0.17Re
29/12 [200/83]
Plate
98Mg-1.25Zn-0.17Re
Magnesium and Magnesium Base Alloys 81
ASTM
B 90
186
M11311
B 90
AZ31B (-O, H24, H26) AZ31C (-O, H24, H26) AZ31C (-O, H24, H26) HK31A (-O, H24)
81
ASTM
B 90
81
ASTM
B 90
81
ASTM
81
ASTM
B 90
HK31A (-O, H24)
M13310
81
ASTM
B 90
HK31A (-O, H24)
M13310
81
ASTM
B 90
ZE10A (-O)
M16100
81
ASTM
B 90
ZE10A (-O)
M16100
81
ASTM
B 90
ZE10A (-O)
M16100
81 81 81 81
ASTM ASTM ASTM ASTM
B 91 B 91 B 107 B 107
AZ31B (-F) AZ61A (-F) AZ31B (-F) AZ31B (-F)
M11311 M11610 M11311 M11311
81
ASTM
B 107
AZ31B (-F)
M11311
81
ASTM
B 107
AZ31B (-F)
M11311
81 81
ASTM ASTM
B 107 B 107
AZ31B (-F) AZ31B (-F)
M11311 M11311
81
ASTM
B 107
AZ31B (-F)
M11311
M11312 M11312 M13310
0.016–3.000 [0.40–80] 0.016–0.060 [0.40–1.50] 0.061–3.000 [1.50–80] 0.016–0.500 [0.40–13] 0.501–1.000 [13–25] 1.001–3.000 [25–80] 0.016–0.060 [0.40–1.50] 0.061–0.250 [1.50–6.3] 0.251–0.500 [6.30–13] — — ≤0.249 [6.30] 0.250–1.499 [6.3–40] 1.500–2.499 [40–60] 2.500–4.999 [60–130] — 0.028–0.250 [0.70–6.3] 0.251–0.750 [6.30–20]
32/15 [221/103] Forgings 35/19 [241/131] Forgings 32/18 [221/124] Extruded Bars, Rods, Profiles & Wires 32/19 [221/131] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn 92.5Mg-6Al-1Zn 95.5Mg-3Al-1Zn 95.5Mg-3Al-1Zn
31/19 [214/131] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn
29/17 [200/117] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn
29/13 [200/90] 29/17 [200/117]
Extruded Hollow Profiles Extruded Tubes
95.5Mg-3Al-1Zn 95.5Mg-3Al-1Zn
29/13 [200/90]
Extruded Tubes
95.5Mg-3Al-1Zn
(Continued)
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Magnesium and Magnesium Base Alloys
187
ASTM ASTM
B 107 B 107
AZ31C (-F) AZ31C (-F)
M11312 M11312
81
ASTM
B 107
AZ31C (-F)
M11312
81
ASTM
B 107
AZ31C (-F)
M11312
81 81
ASTM ASTM
B 107 B 107
AZ31C (-F) AZ31C (-F)
M11312 M11312
81
ASTM
B 107
AZ31C (-F)
M11312
81 81
ASTM ASTM
B 107 B 107
AZ61A (-F) AZ61A (-F)
M11610 M11610
81
ASTM
B 107
AZ61A (-F)
M11610
81 81
ASTM ASTM
B 107 B 107
AZ61A (-F) AZ61A (-F)
M11610 M11610
81 81
ASTM ASTM
B 107 B 107
MlA (-F) MlA (-F)
M15100 M15100
81
ASTM
B 107
MlA (-F)
M15100
81 81
ASTM ASTM
B 107 B 107
MlA (-F) MlA (-F)
M15100 M15100
83 83
ASTM ASTM
B 80 B 80
AZ91C (-F) AZ92A (-F)
M11914 M11920
≤0.249 [6.30] 0.250–1.499 [6.3–40] 1.500–2.499 [40–60] 2.500–4.999 [60–130] — 0.028–0.250 [0.70–6.3] 0.251–0.750 [6.30–20] ≤0.249 [6.30] 0.250–2.499 [6.3–60] 2.500–4.999 [60–130] — 0.028–0.750 [0.70–20] ≤0.249 [6.30] 0.250–2.499 [6.3–60] 2.500–4.999 [60–130] — 0.028–0.750 [0.70–20] — —
32/18 [221/124] Extruded Bars, Rods, Profiles & Wires 32/19 [221/131] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn 95.5Mg-3Al-1Zn
31/19 [214/131] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn
29/17 [200/117] Extruded Bars, Rods, Profiles & Wires
95.5Mg-3Al-1Zn
29/13 [200/90] 29/17 [200/117]
Extruded Hollow Profiles Extruded Tubes
95.5Mg-3Al-1Zn 95.5Mg-3Al-1Zn
29/13 [200/90]
Extruded Tubes
95.5Mg-3Al-1Zn
35/18 [241/124] Extruded Bars, Rods, Profiles & Wires 37/21 [255/145] Extruded Bars, Rods, Profiles & Wires
92.5Mg-6.5Al-1Zn 92.5Mg-6.5Al-1Zn
37/19 [255/131] Extruded Bars, Rods, Profiles & Wires
92.5Mg-6.5Al-1Zn
33/13 [228/90] 33/13 [228/90]
Extruded Hollow Profiles Extruded Tubes
92.5Mg-6.5Al-1Zn 92.5Mg-6.5Al-1Zn
27/– [186/–] 29/– [200/–]
Extruded Bars, Rods, Profiles & Wires Extruded Bars, Rods, Profiles & Wires
98Mg-1.6Mn 98Mg-1.6Mn
26/– [179/–]
Extruded Bars, Rods, Profiles & Wires
98Mg-1.6Mn
25/– [172/–] 25/– [172/–]
Extruded Hollow Profiles Extruded Tubes
98Mg-1.6Mn 98Mg-1.6Mn
21/10 [145/69] 21/10 [145/69]
Sand Castings Sand Castings
90.5Mg-8.7Al-0.7Zn-0.2Mn 88.5Mg-9Al-2Zn
(Continued)
AWS B2.1/B2.1M-BMG:2009
81 81
Material Number Standard
Base Metal Type, Grade, or Specification Alloy Designation
UNS Number
Thickness or Diameter Limitations, in [mm]
Minimum Tensile/Yield Strength, ksi [MPa]
Product Form
Nominal Composition
Sand Castings Permanent Mold Casting Permanent Mold Casting Permanent Mold Casting Investment Castings Investment Castings Investment Castings Investment Castings
99.3Mg-0.6Zr 89.5Mg-10Al-0.2Mn 90.5Mg-8.7Al-0.7Zn-0.2Mn 88.5Mg-9Al-2Zn 89.5Mg-10Al-0.2Mn 90.5Mg-8.7Al-0.7Zn-0.2Mn 88.5Mg-9Al-2Zn 99.3Mg-0.6Zr
Magnesium and Magnesium Base Alloys 83 83 83 83 83 83 83 83
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM
B 80 B 199 B 199 B 199 B 403 B 403 B 403 B 403
KlA (-F) AM100A (-F) AZ91C (-F) AZ92A (-F) AM100A (-F) AZ91C (-F) AZ92A (-F) K1A (-F)
M18010 M10100 M11914 M11920 M10100 M11914 M11920 M18010
— — — — — — — —
22/5 [152/34] 18/9 [124/62] 21/10 [145/69] 21/10 [145/69] 18/9 [124/62] 16/9 [110/62] 18/9 [124/62] 22/5 [152/34]
AWS B2.1/B2.1M-BMG:2009
Table D.2 (Continued) M-Number Listing of Base Metals—Nonferrous Alloys
188
AWS B2.1/B2.1M-BMG:2009
Table D.3 Listing of Base Metal Specifications—Iron Castings
AWS D11.2 Base Metal Group Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Minimum As-Welded Tensile/Yield Strength, ksi [MPa]
Type of Base Metal
Nominal Composition
Iron Castings a, b A A A A A A A A A A A A A A A A A A A A A A A A A A A A A A
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM SAE SAE SAE SAE SAE
A 48 A 48 A 48 A 48 A 48 A 48 A 48 A 48 A 48 A 74 A 126 A 126 A 126 A 159 A 159 A 159 A 159 A 159 A 159 A 159 A 159 A 159 A 319 A 319 A 319 J431 J431 J431 J431 J431
Class 20 Class 25 Class 30 Class 35 Class 40 Class 45 Class 50 Class 55 Class 60 Class A Class A Class B Class C Grade 1800 Grade 2500 Grade 2500a Grade 3000 Grade 3500 Grade 3500b Grade 3500c Grade 4000 Grade 4000d Class I Class II Class III G1800 G2500 G3000 G3500 G4000
F11401 F11701 F12101 F12401 F12801 F13101 F13501 F13801 F14101 — F11501 F12102 F12103 F10004 F10005 F10009 F10006 F10007 F10010 F10011 F10008 F10012 F10001 F10002 F10003 F10004 F10005 F10006 F10007 F10008
20/– [138/–] 25/– [172/–] 30/– [207/–] 35/– [241/–] 40/– [276/–] 45/– [310/–] 50/– [345/–] 55/– [379/–] 60/– [414/–] 21/– [145/–] 21/– [145/–] 31/– [214/–] 41/– [283/–] 18/– [124/–] 25/– [172/–] 25/– [172/–] 30/– [207/–] 35/– [241/–] 35/– [241/–] 35/– [241/–] 40/– [276/–] 40/– [276/–] 25/– [172/–] 30/– [207/–] 40/– [276/–] 18/– [124/–] 25 [172] 30 [207] 35 [241] 40 [276]
Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron Gray Cast Iron
Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified 0.75 Max.P, 0.15 Max.S 0.75 Max.P, 0.15 Max.S 0.75 Max.P, 0.15 Max.S 0.75 Max.P, 0.15 Max.S 0.55Si-0.65Mn; 4.35CE 2.2 Si-0.75Mn; 4.12CE 1.85Si-0.75Mn; 4.12 CE 2.1Si-0/75Mn; 4.02CE 2.0Si-0.75Mn; 3.8CE 1.55Si-0.75Mn; 3.8CE 1.55Si-0.75Mn; 3.8CE 1.95Si-0.85Mn; 3.8CE 1.95Si-0.85Mn; 3.8CE Not Specified Not Specified Not Specified 2.3SI-0.65Mn; 4.35CE 2.3Si-0.75Mn; 4.12CE 2.1Si-0.65Mn; 4.02CE 2.0Si-0.75Mn; 3.8CE 1.95Si-0.95Mn; 3.8CE
B B B B B B B B B B
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM SAE
A 536 A 536 A 536 A 536 A 536 A 716 A 746 A 874 A 897 J434
100-70-03 120-90-02 60-40-18 65-45-12 80-55-06 60-42-10 60-42-10 — 125-80-10 D4018
F34800 F36200 F32800 F33100 F33800 F32900 — — — F32800
100/70 [689/483] 120/90 [827/621] 60/40 [414/276] 65/42 [448/290] 80/55 [552/379] 60/– [414/–] 60/– [414/–] 45/30 [310/207] 125/80 [862/552] 60/– [414/–]
Ductile Ductile Ductile Ductile Ductile Ductile Ductile Ductile Ductile Ductile
Not specified Not specified Not specified Not specified Not specified Not specified Not specified 3.35C-1.75Si 1.0Ni-0.5Cu-0.35Mn-0.015Mo Not specified
189
AWS B2.1/B2.1M-BMG:2009
Table D.3 (Continued) Listing of Base Metal Specifications—Iron Castings
AWS Base Metal D11.2 Group Standard Specification
Type, Grade, or Alloy Designation
UNS Number
Minimum As-Welded Tensile/Yield Strength, ksi [MPa]
Type of Base Metal
Nominal Composition
Iron Castings a, b
a b
B B B
SAE SAE SAE
J434 J434 J434
D4512 D5506 D7003
F33100 F33800 F34800
65/– [448/–] 80/– [552/–] 100/– [689/–]
Ductile Ductile Ductile
Not specified Not specified Not specified
C C C C C C C C C C C C C C C C
ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM ASTM SAE SAE
A 47 A 47 A 197 A 220 A 220 A 220 A 220 A 220 A 220 A 220 A 220 A 602 A 602 A 602 J158a J158a
32510 35018 — 40010 45006 45008 50005 60004 70003 80002 90001 M3210 M4504 M5003 M3210 M4504
F22200 F22400 F22200 F22830 F23131 F23130 F23530 F24130 F24830 F25530 F26230 F20000 F20000 F20000 F20000 F20001
50/– [345/–] 53/– [365/–] 40/– [276/–] 60/– [414/–] 65/– [448/–] 65/– [448/–] 70/– [483/–] 80/– [552/–] 85/– [586/–] 95/– [655/–] 105/– [724/–] 50/– [345/–] 65/– [448/–] 75/– [517/–] 50/– [345/–] 65/– [448/–]
Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable Malleable
Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified Not Specified
In the absence of an M number to group the alloys, a separate procedure qualification is required for each group of the above materials. The groups are based on AWS D11.2.
190