COMPOSITE SHEET FORMING
COMPOSITE MATERIALS SERIES
Series Editor: R. Byron Pipes, Center for Composite Materials, Un...
395 downloads
3051 Views
20MB Size
Report
This content was uploaded by our users and we assume good faith they have the permission to share this book. If you own the copyright to this book and it is wrongfully on our website, we offer a simple DMCA procedure to remove your content from our site. Start by pressing the button below!
Report copyright / DMCA form
COMPOSITE SHEET FORMING
COMPOSITE MATERIALS SERIES
Series Editor: R. Byron Pipes, Center for Composite Materials, University of Delaware, Newark, Delaware, USA Vol. Vol. Vol. Vol. Vol. Vol.
1 2 3 4 5 6
Vol. Vol. Vol. Vol.
7 8 9 10
Friction and Wear of Polymer Composites (K. Friedrich, Editor) Fibre Reinforcements for Composite Materials (A.R. Bunsell, Editor) Textile Structural Composites (T.-W. Chou, Editor) Fatigue of Composite Materials (K.L. Reifsnider, Editor) Interlaminar Response of Composite Materials (N.J. Pagano, Editor) Application of Fracture Mechanics to Composite Materials (K. Friedrich, Editor) Thermoplastic Composite Materials (L.A. Carlsson, Editor) Advances in Composite Tribology (K. Friedrich, Editor) Damage Mechanics of Composite Materials (R. Talreja, Editor) Flow and Rheology in Polymer Composites Manufacturing (S.G. Advani, Editor)
Cover illustration- Arrow diagram for a [0,9012s blister fairing, 61max- 35.3%, (for details see p. 233).
t~Zmax = - 2 5 . 9 %
Composite Materials Series, 11 COMPOSITE SHEET FORMING edited by
D. Bhattacharyya Department of Mechanical Engineering, School of Engineering, University of Auckland, Auckland, New Zealand
1997 ELSEVIER Amsterdam
m
Lausanne
m
New
York
m
Oxford
m
Shannon
--
Tokyo
ELSEVIER SCIENCE B.V. Sara Burgerhartstraat 25 P.O. Box 211, 1000 AE Amsterdam, The Netherlands
ISBN ISBN
0-444-82641-6 (Vol. 11) 0-444-42525-X (Series)
9 1997 Elsevier Science B.V. All rights reserved. No part of this publication may be reproduced, stored in a retrieval system or transmitted in any form or by any means, electronic, mechanical, photocopying, recording or otherwise, without the prior written permission of the publisher, Elsevier Science B.V., Copyright and Permissions Department, P.O. Box 521, 1000 AM Amsterdam, The Netherlands. Special regulations for readers in the U S A - This publication has been registered with the Copyright Clearance Center Inc. (CCC), 222 Rosewood Drive, Danvers, MA 01923. Information can be obtained from the CCC about conditions under which photocopies of parts of this publication may be made in the USA. All other copyright questions, including photocopying outside the USA, should be referred to the copyright owner, Elsevier Science B.V., unless otherwise specified. No responsibility is assumed by the publisher for any injury and/or damage to persons or property as a matter of products liability, negligence or otherwise, or from any use or operation of any methods, products, instructions or ideas contained in the material herein. This book is printed on acid-free paper. Printed in The Netherlands.
PREFACE Sheet forming is one of the most used processes in metal forming and hence it is not surprising to see considerable efforts being put into adapting or modifying the existing sheet metal forming techniques to suit the needs of forming composite sheets. With the increasing availability of various types of fibre-reinforced polymeric sheets, especially with thermoplastic matrices, the scope of using such materials is rapidly expanding in the automobile, building, sports and other manufacturing industries beyond the traditional areas of aerospace and aircraft applications. Their good structural and anti-corrosion properties with available design versatility give them many advantages over traditional metallic sheets. However, to realise the full potential of these materials, it is often necessary to redesign the component with subsequent manufacturing in mind. For economic competitiveness it is also desirable to develop rapid manufacturing techniques suitable for different types of composite sheets. Thus the understanding of their fundamental deformation behaviour, along with the capability of developing analytical models, is essential for efficient and defect-free forming of this relatively new generation of materials. This book contains twelve chapters and attempts to cover different aspects of sheet forming including both thermoplastic and thermosetting materials. In view of the expanded role of fibre-reinforced composite sheets in the industry, the book also describes some non-traditional applications, processes and analytical techniques involving such materials. It has often been noted by the Editor and his research colleagues that familiarity with the basic principles and ideas of sheet metal forming is somewhat lacking among the researchers of composite sheet forming. Although there are fundamental differences in nature between metallic and composite sheets, there are many concepts and techniques, originally developed for sheet metal forming, that can be successfully utilised for composites. Hence the first chapter has been dedicated to a brief introduction to the principles of sheet metal forming. The next two chapters introduce the various forms of materials, manufacturing techniques and the fundamentals of computer simulation. Chapter 4 describes the different aspects of thermoforming of continuous fibre-reinforced thermoplastics and the following chapter studies the shear and frictional behaviour of composite sheets during forming. Grid strain analysis is an established technique for sheet metals; Chapter 6 explores the possibility of applying this method in continuous fibre-reinforced polymeric sheets. For an efficient manufacturing process development, finite element modelling and an understanding of rheology play extremely important roles; the next two chapters address these topics with the fundamental concepts reviewed and the recent developments discussed. Chapter 9 introduces the theory of bending, which is an
vi
Preface
integral mechanism of most sheet forming processes, of thermoplastic composite sheets and shows a novel way of determining both longitudinal and transverse viscosities through vee-bend tests. A significant expansion of the usage of composite materials is taking place in biomedical areas and Chapter 10 discusses the thermoforming of knitted fabric-reinforced thermoplastics for load-bearing, anisotropic bio-implants. Chapter 11 studies the forming of thermoset composites, a new technique of manufacturing composite components, and highlights the phenomenological similarities with those found with thermoplastics. The last chapter introduces roll forming, a commonly used rapid manufacturing process for sheet metals, and discusses the possibility of applying it economically for continuous fibre-reinforced thermoplastic sheets. I would like to thank Dr R. B. Pipes, editor-in-chief of this Elsevier series on composite materials, for inviting me to organise and edit this particular volume. Thanks are also due to the authors of the various chapters for making their learned contributions and complying with the necessary publication schedule. Finally I wish to thank the University of Auckland, the German Science Foundation, the University of Kaiserslautern and my family for their support during my sabbatical leave which allowed me to complete the final phase of the editing work. D. Bhattacharyya
LIST OF CONTRIBUTORS
S.G. ADVANI
Department of Mechanical Engineering, University of Delaware, Newark, DE 19716, USA B. Tomas ASTROM
Department of Aeronautics, Division of Lightweight Structures, Royal Institute of Technology, S-IO0 44 Stockholm, Sweden D. B H A T T A C H A R Y Y A
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand G.R. CHRISTIE
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand T.S. CREASY
Department of Mechanical Engineering, University of Delaware, Newark, DE 19716, USA (currently at University of Southern California, Los Angeles, CA,
USA) J.L. D U N C A N
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand R.J. DYKES
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand K. F R I E D R I C H
Institute for Composite Materials Ltd. (IVW), University of Kaiserslautern, 67663 Kaiserslautern, Germany M.O. G H A F U R
Polydynamics Inc., 1685 Main St. West, Suite 305, Hamilton, Ontario, Canada L8S 1G5 vii
viii
List of contributors
Timothy G U T O W S K I
Laboratory for Manufacturing and Productivity, Massachusetts Institute of Technology, Cambridge, MA 02139, USA M. HOU
Centre for Advanced Materials Technology, Department of Mechanical Engineering, University of Sydney, Sydney, N S W 2006, Australia B.L. K O Z I E Y
Polydynamics Inc., 1685 Main St. West, Suite 305, Hamilton, Ontario, Canada L8S 1G5 J. KREBS
Institute for Composite Materials Ltd. (IVW), University of Kaiserslautern, 67663 Kaiserslautern, Germany Haorong LI
Laboratory for Manufacturing and Productivity, Massachusetts Institute of Technology, Cambridge, MA 02139, USA Patrick J. M A L L O N
Mechanical and Aeronautical Engineering Department, University of Limerick, Limerick City, Ireland S.J. M A N D E R
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand (currently at McKinsey & Company, Sydney, NSW, Australia) T.A. M A R T I N
Composites Research Group, Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand J. M A Y E R
Biocompatible Materials Science and Engineering, Department of Materials, Swiss Federal Institute of Technology, ETH Zurich, Wagistrasse 23, 8952 Schlieren, Switzerland S.P. McENTEE
Composites Research Unit, University College, Galway, Ireland G.B. McGUINNESS
Composites Research Unit, University College, Galway, Ireland F.A. M I R Z A
Faculty of Engineering, McMaster University, Hamilton, Ontario, Canada L8S 4L7
Lbt of contributors
ix
Adrian M. M U R T A G H Engineering Department, Cambridge University, Trumpington Street, Cambridge CB2 1PZ, UK C.M. 6 BR,~DAIGH Composites Research Unit, University College, Galway, Ireland S.M. P A N T O N
Composites Research Group, Department of Mechanical Eng&eer&g, University of Auckland, Private Bag 92019, Auckland, New Zealand S.F. SHULER Department of Mechanical Eng&eering, University of Delaware, Newark, DE 19716, USA (currently at General Electric Co., Pittsfied, MA, USA) J. V L A C H O P O U L O S
Faculty of Eng&eering, McMaster University, Hamilton, Ontario, Canada L8S 4L7 E. W I N T E R M A N T E L
Biocompatible Materials Science and Eng&eering, Department of Materials, Swiss Federal Institute of Technology, ETH Zurich, Wagistrasse 23, 8952 Schlieren, Switzerland
This . Page Intentionally Left Blank
CONTENTS
A more detailed contents list is given at the beginning of each chapter.
Preface
v
List of Contributors
vii
Chapter 1 (J.L. Duncan and S.M. Panton) Introduction to sheet metal forming
1
Abstract 1 1.1. Introduction 2 1.2 Introduction to plastic flow theory 2 1.3. Forming characteristics of sheet metals 1.4. Forming limits for sheet metal 12 1.5. Industrial sheet metal forming 15 1.6. Bending and spring-back 19 1.7. Superplasticity 23 References 25
Chapter 2 (B. Tomas Astr6m) Thermoplastic composite sheet forming: materials and manufacturing techniques Abstract 27 2.1. Introduction 28 2.2. Constituents 29 2.3. Properties 48 2.4. Manufacturing techniques Acknowledgement 72 References 72
60
xi
27
Contents
xii
Chapter 3 (B.L. Koziey, M.O. Ghafur, J. Vlachopoulos and F.A. Mirza)
Computer simulation of thermoforming 75 Abstract 75 3.1. Introduction 76 3.2. Sheet production 77 3.3. Thermoforming simulation 3.4. Concluding remarks 88 References 88
78
Chapter 4 (K. Friedrich, M. Hou and J. Krebs)
Thermoforming of continuous fibre/thermoplastic composite sheets Abstract 92 4.1. Introduction 92 4.2. Experimental details and procedures 96 4.3. 2-D stamp forming 100 4.4. 3-D stamp forming 137 4.5. 3-D diaphragm forming of GF/PP laminates 4.6. Summary 159 Acknowledgements 160 References 160
91
146
Chapter 5 (A.M. Murtagh and P.J. Mallon)
Characterisation of shearing and frictional behaviour during sheet forming Abstract 163 5.1. Introduction 164 5.2. Transverse fibre flow 170 5.3. Intra-ply shear 173 5.4. Inter-ply slip 177 5.5. Friction during thermoforming References 214
197
Chapter 6 (T.A. Martin, G.R. Christie and D. Bhattacharyya)
Grid strain analysis and its application in composite sheet forming 217 Abstract 217 6.1. Introduction 218 6.2. Large strain analysis 218 6.3. Method of least squares fitting 224 6.4. Forming a composite spherical dome
226
163
Contents
xiii
6.5. Forming a composite blister fairing 230 6.6. Draping theory of textile fabrics 234 6.7. Diagnostic applications 238 6.8. Concluding remarks 241 References 244
Chapter 7 (C.M. O Brfidaigh, G.B. McGuinness and S.P. McEntee) Implicit finite element modelling of composites sheet forming processes
247
Abstract 248 7.1. Introduction 248 7.2. Modelling of composite sheets during forming 254 7.3. Numerical s o l u t i o n s - plane stress problems 258 7.4. Central indentation of a composite sheet ~ the shear-buckling problem 7.5. Experimental comparisons - - diaphragm forming 286 7.6. Conclusions of plane stress analysis 303 7.7. Numerical s o l u t i o n s - plane deformation problems 305 7.8. Conclusions of plane deformation analysis 315 Acknowledgements 318 Nomenclature 318 References 319
Chapter 8 (S.G. Advani, T.S. Creasy and S.F. Shuler) Rheology of long fiber-reinforced composites in sheet forming
323
Abstract 324 8.1. Introduction 324 8.2. Rheological properties 329 8.3. Rheological measurement techniques 348 8.4. Why the rheological properties are important and how to use them in sheet forming 356 8.5. Outlook 366 References 367
Chapter 9 (T.A. Martin, S.J. Mander, R.J. Dykes and D. Bhattacharyya) Bending of continuous fibre-reinforced thermoplastic sheets Abstract 371 9.1. Introduction 372 9.2. Development of an idealised viscous bending model 9.3. Experimental procedures 380
371
374
263
xiv
Contents
9.4. Results and discussion 382 9.5. Modified constant shear rate tests 9.6. Conclusions 399 Acknowledgements 399 References 400
392
Chapter 10 (J. Mayer and E. Wintermantel) Thermoforming processes for knitted-fabric-reinforced thermoplastics: new manufacturing techniques for load-bearing, anisotropic implants 403 Abstract 404 10.1. General aspects of anisotropic biomaterials for load-bearing implants 10.2. Knitted-carbon-fiber-reinforced composite materials 405 10.3. Net-shape forming of knitted fabrics for load-transmitting implants shown for an ulnar osteosynthesis plate 419 10.4. Deep drawing of knitted-fiber-reinforced organo-sheets 428 10.5. Discussion 432 10.6. Summary and conclusions 435 Acknowledgements 435 References 436
Chapter 11 (H. Li and T. Gutowski) The forming of thermoset composites
441
Abstract 441 11.1. Introduction to thermoset forming 442 11.2. Kinematics 446 11.3. Thermoset forming experiments and forming limit analysis 11.4. Concluding remarks 468 References 471
455
Chapter 12 (S.J. Mander, S.M. Panton, R.J. Dykes and D. Bhattacharyya) Roll forming of sheet materials
473
Abstract 474 12.1. Introduction 474 12.2. Roll forming equipment and tooling 476 12.3. Conventional form roll design 483 12.4. Computer-aided design in roll forming 489 12.5. Deformation analysis of roll forming 491
404
Contents
12.6. Roll forming of thermoplastic material 12.7. Concluding remarks 512 Acknowledgements 513 References 513 Author Index Subject Index
517 525
xv
498
This . Page Intentionally Left Blank
Composite Sheet Forming edited by D. Bhattacharyya 9 Elsevier Science B.V. All rights reserved.
Chapter 1
Introduction to Sheet Metal Forming J.L. D U N C A N and S.M. P A N T O N Department of Mechanical Engineering, University of Auckland, Private Bag 92019, Auckland, New Zealand
Contents Abstract 1 1.1. Introduction 2 1.2. Introduction to plastic flow theory 2 1.2.1. The principal element 2 1.2.2. Yielding of isotropic materials 2 1.2.3. Yielding of anisotropic materials 3 1.2.4. Deformation of principal element 4 1.2.5. Deviatoric stresses 5 1.2.6. The flow rule 5 1.2.7. Anisotropic flow rules 6 1.2.8. Plastic work 6 1.3. Forming characteristics of sheet metals 6 1.3.1. Approximate constitutive relationships 11 1.3.2. The relation between tensile data and multiaxial stress conditions 1.4. Forming limits for sheet metal 12 1.5. Industrial sheet metal forming 15 1.5.1. Stretch forming 15 1.5.2. Deep drawing 17 1.6. Bending and spring-back 19 1.6.1. Bending without tension 19 1.6.2. Bending under tension 22 1.7. Superplasticity 23 References 25
11
Abstract
This chapter is intended to provide a concise introduction to plastic flow theory and the mechanics of sheet metal forming. The influence of material properties on sheet metal "formability" is considered with specific reference to the properties that can be determined from a simple tensile test. The instabilities which limit different forming operations are described and the forming limit diagram introduced. Simple
2
J.L. Duncan and S.M. Panton
models are derived for some practical forming processes, and the forming conditions that result are described. A brief introduction to superplastic forming is given.
1.1. Introduction Sheet metal forming covers a wide variety of operations and consequently many different forming conditions. If we consider a small element of the sheet, as shown in fig. 1.1, it is observed that there are a number of common factors in the state of stress and strain in most of these processes. These can be summarised in the following way: 1. the sheet is formed by tractions transmitted through the sheet; 2. at least one principal stress is tensile; 3. with very few exceptions, the through thickness stress is zero and consequently a state of plane stress exists; 4. the process is limited by the instabilities of local necking or wrinkling (buckling). In this chapter, we first give an introduction to sheet metal forming and in section 1.2 look at some fundamentals of plastic flow theory which is the basis for studying the mechanics of forming. In section 1.3, we examine how the material properties of sheet metal can be described in a way that helps to characterise the formability of the sheet material. In section 1.4, the instabilities which limit the different sheet forming operations will be examined and in section 1.5, we develop simple models for some practical forming processes.
1.2. Introduction to plastic flow theory 1.2.1. The principal element
The state of stress at a point can be expressed in terms of the magnitude and orientation of three principal stresses as shown in fig. 1.2; in what follows, cr3, is the stress normal to the sheet, which, as mentioned, is usually zero. 1.2.2. Yielding of isotropic materials
Plastic yielding is the transition from small and recoverable elastic deformation to irreversible, permanent deformation. In a uniaxial test, the instantaneous value of the yield stress is referred to as the flow stress, of.
Fig. 1.1. A small element taken from a deforming sheet.
Introduction to sheet metal form&g
3
O3
(Yl
(Y2
Fig. 1.2. The principal stresses at a point.
Two well-known criteria for the onset of plastic yielding are (i) the Tresca and (ii) the von Mises yield criteria. The Tresca yield criterion states that yielding will commence when the magnitude of the maximum shear stress is equivalent to the maximum shear stress at yield in a uniaxial test. Relating the maximum shear stress to the principal stresses through Mohr's circle of stress, it can be shown that Tresca's yield criterion can be stated in terms of the principal stresses and the flow stress, 0"1 --0"3 = O f
(1.1)
for the case of al > a2 > a3. As originally stated, the von Mises criterion was based on the assumption that the distortional strain energy in a general state of stress reaches a critical value at yield. One could, however, state that yielding occurs at a critical value of the root-meansquare average of the the maximum shear stresses in an element. This gives the same result, which can be expressed mathematically as (0-1 -- 0"2) 2 "+- (0"1 -- 0"2) 2 + (0"1 -- 0"2) 2 = 20-2
(1.2)
It may be seen from either criterion that in metals, yielding is fundamentally related to the shear stresses in an element and that there is not a great difference between the two criteria. The stress conditions in sheet metal forming are generally those of plane stress and the two criteria can be compared graphically in fig. 1.3. It may be noted that each gives identical results for conditions of uniaxial stress and equal biaxial stress, but for other conditions the von Mises yield criterion predicts higher stresses for the onset of yielding.
1.2.3. Yielding of anisotropic mater&& In the above section, it was assumed that yielding is independent of the orientation of the principal axes. In anisotropic materials this assumption is not valid. A common form of anisotropy is for the material properties in the thickness direction to vary from those in the plane of the sheet. This type of variation of material properties with direction can be characterised by the constant, R which is the ratio of width
4
J.L. Duncan and S.M. Panton
(Yl Tresca
i,,
__.
if2
V
_ h .
Mises
Fig. 1.3. Comparison of the Tresca and von Mises yield criteria
to thickness strain in a uniaxial tensile test. In this case a suggested plane stress yield locus [1] is (1.3)
O'~ + O'~ + R(ff 1 --if2) a = R(o'f) a
where a is a constant related to the crystal structure of the material (typically about 6 for body-centred cubic materials and 8-10 for face-centred cubic materials). 1.2.4. Deformation of a principal element
A principal element will deform without shear and the strain increments which result are principal ones. With reference to fig. 1.4, the strain increments are, de1
-
da/a
(1.4)
de 2 - db/b de1 - dc/c
A metal deforming elastically undergoes a small volumetric change; during plastic strain, however, the volume change in a typical metal is very small and is often neglected. Therefore, (a + da)(b + db)(c + dc) - abc - 0 2
2
c+~
1
3
1"~
Fig. 1.4. Deformation of a principal element.
~
"~3
Introduction to sheet metal forming
5
Neglecting the product terms of small quantities one obtains da/a + db/b + de/c = 0 so that the sum of the principal strain increments is zero, i.e. (1.5)
del + de2 + de3 = 0 1.2.5. Deviatoric stresses
The principal stresses may be considered as the sum of two components, namely the hydrostatic stress (o"h) and the deviatoric stresses 0"{, 0"~ 0"~ as shown in fig. 1.5. This leads to the following expressions for the deviatoric stresses 0"~ -- 0"1 - 0"h l 0"2 - - 0"2 -- 0-h
0"~ - 0"3 - 0"h
(1.6)
where 0"h = (0-1 + 0"2 + 0"3)/3. 1.2.6. The flow rule The relation between stress and the strain increment during plastic deformation of isotropic materials is given by the flow rule, (1.7)
de]/0"{ - d e 2 / 0 " 2 ' - d e 3 / 0 " 3 ' - d~.
i.e. the principal strain increments are in the same proportion as the deviatoric stresses, .
!
del "de2"de3
/
/
(1.8a)
"0-1 " 0 2 " 0 3
The constant, d)~, indicates the magnitude of the strain increments and and its value is not determined by the stress state. For a given yielding state of stress, the material may not deform, in which case 3~ -- 0 or in a non-strain-hardening material it may deform appreciably at constant stress. In this respect, plastic deformation differs considerably from the elastic state where there is a one-to-one relationship between stress and strain. Furthermore the same strain state, del, de2, de3 may arise from a number of different stress states which differ only in their hydrostatic component. t
~3
03 IL
~h
+
-
t
Ot
a2
Fig. 1.5. Deviatoric and hydrostatic stresses.
02 ~h
~h
6
J.L. Duncan and S.M. Panton
1.2.7. Anisotropic flow rules
An alternative interpretation of the flow rules is that the vector representing the plastic strain increments is normal to the yield surface (the principle of normality). It follows that in addition to the flow rules described in (1.8a), there are flow rules which correspond to the anisotropic yield criteria described in eq. (1.3). For a situation of plane stress, the anisotropic equivalent of eq. (1.8a) is given [1] by: d e 1 " d e 2 "" (0"1) a - 1 - R ( f f 1 - 0 " 2 ) a - 1 " (0"2) a - 1 -
R(cr 2 -0"1) a-1
(1.8b)
1.2.8. Plastic work
The forces acting on the faces of the principal element shown in fig. 1.4 are ~r1.bc, crz.ac and a3.ab, hence the work done in deforming the element is given by d W = er1bc. da + ~rzac. db + cr3ab, dc
As the volume of the element is abc, from eq. (1.4) we can show that the work done per unit volume is dW/vol = eqdel + crzde2 + cr3de3
(1.9)
This may be rewritten in the form, d W/vol = a . de
(1.1 O)
where a is a generalised stress function called the equivalent, representative or effective stress and de is the equivalent or effective strain increment. It can be shown, using plastic incompressibility and the flow rules, that O" - - 1[(0" 1 -- 0"2) 2 -+" (0" 2 -- 0"3) 2 q- (0" 1 -- 0"3)2]) 0.5
(1.1 la)
and, if the element is deforming, O" : O f
(1.11b)
The equivalent strain increment is de
- - ( 2 [ ( 8 1 - 82) 2 + (82 - 83) 2 -q- (g 1 - 63)2]) 0.5
(1.12)
The equivalent stress and equivalent strain permit material properties determined from a uniaxial test to be applied in problems involving general states of stress. 1.3. Forming characteristics of sheet metals
The most basic test to characterise material behaviour is the tensile test, fig. 1.6. In this section we describe information which can be determined from this test, and explain how it may be related to other stress states which exist in practical forming operations. In the tensile test, a testpiece with a known cross-sectional area and gauge length is subjected to an increasing tensile load until the specimen fails. The extension of the
Introduction to sheet metal forming
7
F
T
[ " I]
i
Lgth
Gauge ~ 1
Currentx-sectional area= A
t [ 1
Originalx-seetior~l area = A o
T
engineering strain = 8L / L
F
truestrain= In ((L+b'I_.)/L) engineering stress= F / A o true stress = F / A
. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . .
Fig. 1.6. Tensile test. gauge length, 8L, is recorded for a given load, F From this information, the engineering stress-engineering strain curve and the true stress-true strain curve may be determined. Initially we consider the engineering stress-strain curve. Different metals exhibit vastly differing stress-strain characteristics, but one may identify three or four distinct regions in the engineering stress-strain curve, fig. 1.7 illustrates the following regions. R e g i o n I. In this region of the stress-strain curve, the deformation is approximately uniform throughout the gauge length and the material remains elastic. The stressstrain relationship is linear and if the load were removed the specimen would return to its original length. In metals, the extension at the limit of elasticity is typically about one part in one thousand. Compared with other materials such as stone or concrete, metals and their alloys have a high stiffness and when they are compared with composites such as wood or with most plastics, they are very stiff. R e g i o n II. Eventually the elastic limit will be reached and the material will begin to
yield plastically. The behaviour of the material in the vicinity of the yield point is complex; however, in fig. 1.8 we observe two distinct types: (a) discontinuous and (b) H'
IH
IV
i i ! i
1 i
', |
,
i
Fig. 1.7. Engineering stress-strain curve.
8
J.L. Duncan and S.M. Panton
(a)
0,)
Fig. 1.8. (a) Discontinuous and (b) continuous yield point phenomena.
continuous yielding. Discontinuous yielding is associated with ageing and with ludering, in which bands of plastically yielded material become visually apparent within regions which are predominantly elastic. Region III. Beyond the elastic limit and any discontinuous stage, the material will deform plastically and in a homogeneous fashion. The increase in the flow stress of the material during this period is known as work-hardening; however, the crosssectional area also decreases so that the engineering stress-strain curve does not give an accurate picture of the rate of hardening. Region IV. Eventually a point will be reached on the stress-strain curve at which the engineering stress reaches a maximum. Beyond this point, small imperfections will act as initiation sites for necking. Deformation will be concentrated in these regions and eventually lead to failure of the strip. We describe this process in more detail in section 1.4. When interpreting a stress-strain curve, there are various pieces of information which can be observed routinely; these are illustrated in fig. 1.9 and are: 9 yield strength indicating the limit of elastic deformation; 9 the work-hardening characteristic of the material which can be quantified by the ratio of the ultimate tensile strength (UTS) to the yield strength, af; 9 the elastic elongation; 9 the yield point elongation, if present; 9 the maximum uniform elongation Total elongation is a widely used technological indicator of the ability of the material to stretch, but some care must be exercised because this is a function not only of material behaviour but also of specimen geometry. In the same material, shorter, wider testpieces will give greater total elongation than long, narrow ones. As we apply a tensile force to a specimen, there will be strain not only in the axial direction, but also in the width and thickness directions. For an isotropic material, these transverse strains would be equal; prior processing of the sheet may result, however, in directional material properties, and these are characterised by the ratio of width strain to thickness strain as shown in fig. 1.10. This has been denoted by, R, in eq. (1.3) above and it is also known as the r-value. It may be noted that a high rvalue will tend to retard the thinning of the material under tension.
Introduction to sheet metal forming
9
Work Hardening UTS / YS typically in the range of
1.2- 2.5 Yield strength typically 150-600 MPa
v
Maximum uniform elongation
l ~ ~ e elongation typically ~ II-"1 around0.1-0.3% II ~ yield point elongation [ I ifpresent
To tal Elongation
Fig. 1.9. A typical engineering stress-strain curve for metals and alloys. F
Thickness
Width
r = width strain / thickness strain
Typically Steels I to 2.5 Aluminium 0.6 to 1.0
F Fig. 1.10. Determination of r-value.
In fig. 1.6, we refer to both true stress-strain and engineering stress-strain curves. The engineering curve is widely used, particularly in specifying material properties. In modelling and analysing the mechanics of sheet forming processes, it is necessary to use the true stress-strain curve. The distinction is as follows. As the specimen will strain in the width and thickness directions as well as axially, the cross-sectional area of the specimen will change; the true stress (the axial load divided by the current cross-sectional) area will differ from the engineering stress (the axial load divided by the original cross-section) particularly when the extension increases to 10% or more. We may also note that for any increase in load, the true strain increment is the resulting change in length divided by the current length (as opposed to the
10
J.L. Duncan and S.M. Panton
engineering strain increment which is the resulting change in length divided by the original length). If we integrate the true strain increments we obtain true strain defined as;
e~- f de- f dL/L-ln(L/Lo)
(1.13)
If we plot true stress against true strain, fig. 1.11, we see a curve that is very different from the engineering stress-strain diagram; it shows that strain hardening continues at a diminishing rate, but it does not cease at the maximum load. One characteristic of sheet metal behaviour that is often referred to is "formability". There is no precise definition of formability as in general usage, it is taken to mean the response of a particular material to a given forming process; this response is often measured in terms of the percentage of rejects in running the sheet in the press shop. As formability depends on the material, the type of deformation process and the state of the tooling used, it is not a single-valued quantity for any batch of sheet. Variability is a major factor in the perceived formability, but apart from this, the measurable properties that can be derived from the tensile test which are considered to enhance formability are: 9 high strain hardening as indicated by the UTS/yield ratio or the slope of the true stress-strain curve; 9 resistance to thinning in terms of a high r-value. Typical values of these properties are given in table 1.1 for different grades of steel sheet commonly used in sheet metal forming. In general, discontinuous yielding and yield point elongation diminish formability and the effects of temperature and strain rate may also need to be considered.
"
w
g Fig. 1.11. True stress-strain curve. TABLE 1.1 Typical material properties for cold-rolled, low-strength steel Commercial quality
Drawing quality (DQ)
DQ special killed
Interstitial free
230 320 1.35 0.20 1.0 30-35
200 310 1.55 0.21 1.2-1.5 38-42
180 300 1.75 0.22 1.6-1.8 40-45
150 320 2.25 0.24 2.0-2.2 45-48
Yield strength (MPa) Ultimate tensile strength (MPa) UTS / YS n r Total elongation (%)
Introduction to sheet metal forming
11
1.3.1. Approximate constitutive relationships
In this section we will look at simple approximations to the uniaxial stress-strain curve. Figure 1.12a shows a rigid-perfectly plastic approximation which is particularly useful for approximate load calculations. In fig. 1.12b, we consider an elasticperfectly plastic model used in studying small strain processes such as bending and springback. In fig. 1.12c, a power hardening law has been fitted to the true stresstrue strain curve over the plastic range. In terms of the uniaxial stress and strain, this can be expressed as (1.14)
al = Ke'~
where K is a coefficient indicating the strength of the material and n is the strain hardening index. It is found that this expression will fit true stress-strain curves of annealed sheet very well except at very low values of strain near initial yielding. In fig. 1.12d, we see a model for the stress-strain-rate characteristics of strain-rate sensitive materials such as superplastic alloys. These empirical relations are presented in order to show that tensile test results, although containing much data, can be summarised by simple models; in certain situations even a model as simple as the rigid-perfectly plastic may give quite acceptable results.
1.3.2. The relation between tensile data and multiaxial stress conditions
The uniaxial stress-strain properties determined from tensile testing as shown in fig. 1.13 can be used in the analysis of the multiaxial stress conditions in general sheet forming operations. In the elastic region (I) the stress-strain characteristics are defined by the wellknown generalised Hooke's laws. The pertinent material properties are Young's modulus and Poisson's ratio. o=-Ke"
v v
o
Log o
(b)
e "-
Bi~m
(d) Log t
Fig. 1.12. Approximate constitutive relationships: (a) Rigidly perfectly plastic, (b) elastic-perfectly plastic, (c) power hardening, (d) non-Newtonian fluid.
12
.
J.L. Duncan and S.M. Panton
.
t,f
.
|~
~Work Hardening/
(II) C,e.,neralised - I Hooke's l (I)
a
-[ w
s
~ "
Fig. 1.13. Relating tensile test data to multiaxial states of stress. The conditions for initial yield (II) are determined using either of the yield criteria described in section 1.2. In the plastic region (III) the stress conditions continue to satisfy the yield criterion and the generalised stress function, a, is equal in magnitude to the instantaneous value of the uniaxial yield strength, i.e. the flow stress of the material, af. The strains in the uniaxial and generalised process are el and e as defined above. For an isotropic material, the generalised stress-strain curve and the uniaxial curve are identical. 1.4. F o r m i n g
l i m i t s for s h e e t m e t a l
The forming of sheet metal is limited by two types of instability, tensile instability (necking) and wrinkling (buckling). In any sheet material, there will always be imperfections in the form of areas which are slightly thinner or weaker than the surrounding sheet. These form the focus of potential necks and we consider first a small geometric imperfection in a tensile test as shown in fig. 1.14. The reduction in the cross-sectional area causes a greater stress in this locality and hence a greater strain; the increased strain will reduce the crosssectional area. The deformation of the whole testpiece will remain stable so long as the force required to deform the imperfection continues to increase with extension of the specimen. At some point, the increase in strength due to strain hardening will be overcome by the reduction in cross-sectional area and deformation will become unstable. For an incompressible material, it can be shown that this occurs when dal/de1 <
O"1
AreaA+~iA ~
F
~
Area A "
Fig. 1.14. Deformation in a tensile test in the presence of a geometric imperfection.
Introduction to sheet metal forming
13
which, for a strain-hardening material obeying the power hardening law, t 7 1 - - Ke~, occurs when, e > n In the tensile strip, a neck will develop at this point which will cover a region in length roughly equal to the width of the specimen. This is termed a diffuse neck. Once a neck has developed, extension of the testpiece is accommodated by deformation in the neck; this causes an increase in the local strain-rate and with ratesensitive materials the development of necking is slowed and it becomes more diffuse. For materials having the kind of behaviour modelled in fig. 1.12d with high "m" values, such as superplastic alloys, this effect is large and the rate of growth of a neck in a material is imperceptible. In such situations, the strip stretches in a nearly uniform manner giving the useful property of permitting high strains. It is stated above that diffuse necking is associated with a maximum in the load carrying capacity of a region of the testpiece, i.e. the product of stress, trl, and area, A, reaches a maximum. Some non-metals, such as certain polymers, have a stressstrain relation which is convex upwards, as shown in fig. 1.15; the same load can be sustained at the initiation of diffuse necking at A as at B. Deformation is therefore only unstable between these points and the neck will draw out until conditions reach the point B and then the neck will travel along the testpiece in a stable manner. This phenomenon is not seen in metals although, in aged materials, Ltider's bands will travel along the strip in a roughly analogous manner. In general sheet forming processes, a diffuse neck is prevented from developing by the constraint of the surrounding material; therefore the sheet will strain in a quasistable manner until a local neck or groove develops with a width of the order of the sheet thickness, as shown in fig. 1.16. If one of the principal strains in the plane of the sheet is zero or negative, then there is a direction of zero extension in the sheet. A ." Constant 10ad line
i3
Fig. 1.15. Stress-strain curve for a polymer which will deform by drawing out a neck.
Fig. 1.16. Imperfection in a continuous sheet.
14
J.L. Duncan and S.M. Panton
local neck, as postulated by Hill [2], is most likely to develop in this direction when the strains satisfy the relation,
(1.15)
81 + 8 2 -" n
If both of the principal strains are tensile, then there is no direction of zero strain. In this case, the Marciniak model [3] shows that the shape of the yield locus can stabilise the process so that necking is delayed. The Hill and Marciniak models when combined give rise to a line in the strain diagram, fig. 1.17, which indicates the onset of local necking. This is called the "forming limit curve". The existence of this curve can also be established experimentally; the standard procedure is to form strips of various width over a hemispherical punch and observe the strain at which necking occurs by use of a circular grid. The use of differing strip widths creates strain conditions which vary from plane strain through to biaxial tension. The whole diagram, fig. 1.17, is commonly known as the "forming limit diagram" and it is widely used in the diagnosis of sheet forming problems. Strains in various regions of the sheet can be measured using some gridding technique and plotted in this diagram. As an example, a typical draw die operation as shown in fig. 1.18, the sheet is clamped around the edge and drawn in by the action of the punch. When the punch bottoms in the die, the region in the centre of the sheet will be stretched in biaxial tension as shown. In the side walls, the sheet is stretched in plane strain while
Hill
Major Principal Strain A E1
Marciniak
El+ez=n
.
9
Biaxial
Tension
/
s t I, s s, f ,,,
Minor Principal Strain
Fig. 1.17. Forming limits imposed by necking.
Stretc~ng
Plane Strain
Drawing Fig. 1.18. Press forming (with draw die).
Introduction to sheet metal forming
15
in the corners, the sheet is stretched in the radial direction and compressed circumferentially. A grid circle at each of these regions will be deformed as shown in fig. 1.19 and the strains in the part will fall within the envelope shown. The importance of leaving a safety zone between this envelope and the forming limit curve is clear. It should be accepted as inevitable that small variations in process characteristics such as friction will cause some variation in strain, and if this variation in strain causes failure of the parts, then the process should be considered incapable. For this reason the forming limit diagram is.an important process control tool. The forming limit diagram is also an important tool during die try-out and can indicate appropriate modifications to the tooling. In general, these modifications will attempt to pull the critical strains away from the forming limit curve for the material.
1.5. Industrial sheet metal forming Industrial applications cover a wide spectrum of processes and, as shown in fig. 1.18, in any one process different regions will have different straining paths. It is not possible here to deal with the whole range of industrial forming operations, but it is useful to look at the idealised cases that exist at either end of this s p e c t r u m - these are two-dimensional stretch forming and axisymmetric deep drawing. The basic mechanics of each will be introduced and from this it is possible to identify the kind of material behaviour that is most advantageous for the particular operation.
1.5.1. Stretch forming In forming shallow, smoothly contoured shells such as autobody panels the sheet is stretched over a punch in a double-acting press as illustrated in the twodimensional model in fig. 1.20. The strains necessary to achieve the desired shape Plane Strain
Equal Biaxial
, s
Drawing
""
""
(Shear)
Typical envelope of strains in a formed part Fig. 1.19. Typical envelope of strains on a forming limit diagram.
16
J.L. Duncan and S.M. Panton
Fig. 1.20. Two-dimensionalmodel of stretch forming. are often quite small, but in order to ensure that the shape of the part is properly fixed without excessive spring-back and in some cases to gain strength in the part by strain hardening the sheet, the strains are often much greater than those required just by geometry. In this type of forming, the part required is contained within the trim line shown; the edges of the sheet under the blankholder are used to provide the appropriate tension to stretch the sheet over the punch and this material is discarded after trimming. The restraint at the flange is created in two ways: one is by friction between the sheet and the blankholder and the other by means of the draw bead shown. In a draw bead, the sheet is bent and unbent as it passes through the bead; the plastic work done results in additional tension on the downstream side. The difference between the two methods of restraining the sheet is that the friction effect will depend on both the coefficient of friction and the blankholder force while the draw bead will create a tension which is proportional to the yield stress and the thickness of the sheet, as may be inferred from section 1.6. In a three-dimensional stretch forming die, the important feature is that the flange is not clamped rigidly, but is allowed to move inward in a controlled fashion. In order to obtain sufficient tension to stretch the sheet over the punch, the tension in the side wall between the blankholder and the punch must be very high and to prevent tearing here the material must have good strain-hardening properties. In the two-dimensional case, the minimum strain will be at the centreline. Due to friction between the sheet and the punch, the tension will build up away from the centre. The equation governing this behaviour can be summarised with the aid of fig. 1.21. If the sheet element subtends an angle, d4~, and is being stretched by a tension, T, (force per unit length in a direction perpendicular to the plane of the diagram), then equilibrium in the radial direction gives that q = T/R
(1.16)
where, q, is the tool contact pressure and R the local radius of curvature of the tool. In the tangential direction, dT --/zq. Rd~b = / z T . dq~
(1.17)
The tension in the sheet is T -- tcr
(1.18)
Introduction to sheet metal forming
17
Fig. 1.21. Element of a sheet being stretched over a punch.
Differentiating and substituting, we obtain
d T / T =/x(dcr/~r + dt/t) dqb
(1.19)
The first term in the brackets in eq. (1.19) is the rate of strain hardening and the second term is the rate of thinning. In order to obtain good stretching over the punch without excessive thinning in the most highly stressed regions, we require a low coefficient of friction and good strain hardening. The latter requirement often means that the sheet must be in a fully annealed condition and referring to table 1.1, it is clear that IF steel will behave well in this application. (In this case, formability is traded off against strength as well as cost.)
1.5.2. Deep drawing In drawing an axisymmetric cup as shown in fig. 1.22, most of the deformation takes place in the outer region or flange which is drawn in to create the cylindrical walls of the cup. The blankholder is used to keep the flange flat and avoid wrinkling; some frictional restraint is inevitable but this is kept a small as possible.
To
BlankH o l ~
Punch ]
--~..T,+OT,
Die
To (a)
Fig. 1.22. Deep drawing a cylindrical cup.
(b)
18
J.L. Duncan and S.M. Panton
The equilibrium equation for an element in the flange shown in fig. 1.22b is
dT~o To-T~o= T~
r
0
(1.20)
The stress state in the flange is illustrated in the yield locus in fig. 1.23a. At the outside, A, a state of uniaxial compression will exist; at the inner part of the flange, B, the radial tension, T~, causes the radial stress to approach the yield stress in uniaxial tension, ~rf. The corresponding strain paths are shown in fig. 1.23b. It may be seen that the strains in the centre of the part are small, indicating that in deep drawing most of the deformation is confined to the flange. The forming limit curve is also shown in this diagram and it will be seen that necking is unlikely to limit the process. Furthermore as the level of the forming limit curve depends on the strain-hardening index, n, a low value of n can be accommodated and it is possible to deep draw fully cold-worked sheet. In the diagram in fig. 1.23b, the left-hand diagonal is a path of constant thickness deformation; in drawing the flange, its thickness will be unchanged or slightly increased. It may also be shown that a high r-value is advantageous in deep drawing as it increases the strength of the cup wall, which would deform by stretching and thinning, and decrease the strength of the flange. This brief examination of two idealised processes at the extremes of the spectrum of practical forming operations shows that different material properties such as the strain-hardening index, n, and the normal anisotropy ratio, the r-value, influence different processeses in different ways. In general, the magnitude of the tractions or tension that is developed in the sheet can be understood by examining the loading
r,
A
(a)
Fig. 1.23. Axisymmetricdeep drawing.
TO
(b)
Introduction to sheet metal forming
19
paths in a stress diagram such as fig. 1.23a and the deformation of the sheet and the limits imposed by necking anticipated from the forming limit diagram, as in fig. 1.23b. 1.6. Bending and spring-back Sheet bending is generally considered as a plane strain-plane stress process and the variables are indicated in fig. 1.24. The moment, M, and the tension, T, are values per unit length along the bend. Except for very small radius bends, the strain distribution is assumed to be linear, i.e. el - ln(1 + y/R)
(1.21)
where y is the distance from the neutral axis. Since y/R is small, el is approximately equal to y/R [4].
1.6.1. Bending without tension The neutral axis is at the mid-plane, and the strain distribution is as shown in fig. 1.25. The stress distribution depends on the stress-strain relationship for the material, and it is convenient to express this in terms of the major stress and strain, i.e. 0"1 = f(el) (82
(1.22)
- - 0" 3 - - 0 ) .
z"
~.':.~~~..-~:
t~2
....
9
t
/
,'-,'l
"
'~,~',,
-:'~::~:~:~.:~
"
_
"
,4
"l
/ I / s /
I / I
I
/
',.
0
." R
." /
I 9
/
I
Fig. 1.24. Variables in sheet bending.
, ; : ~
M
20
J.L. Duncan and S.M. Panton 01 - E'81
M
~
,~ 9
(Plastic/ power hardening)
Fig. 1.25. Stress and strain distributions in bending. For an elastic-perfectly plastic material: (i) the stress in the elastic region is given by or1 = E ' e l
(1.23)
where E ' = E/(1 - v 2) and v is Poisson's ratio. (ii) the stress in the plastic region is given by o1 = S
(1.24)
where for a perfectly plastic, von Mises material of constant flow stress, S is related to the flow stress (~rf) by S = (4/3) ~ If the material is elastic, the following well-known equation applies M I I = cqly = E ' I R
(1.25)
At the limiting elastic curvature, ~r1 = S at y = t/2 and hence the limiting elastic curvature and the corresponding moment are given by, (1/R)E -- 2 S / E ' t , ME -- St2/6
(1.26)
As the curvature increases, the material will progressively contain more material in the plastic region, fig. 1.26. From the right-hand drawing of fig. 1.26c, the fully plastic moment, can be determined as Mp = St2/4
(1.27)
A typical moment-curvature characteristic is shown in fig. 1.27. It may be noted that as Mp = 1.5ME, the change in curvature upon unloading A(1/R) = 1.5 (1/R)E. Hence A(1/R) = 3S/E't
(1.28)
Introduction to sheet metal forming
21
Increasing Moment v
PI
.Elastic
M,
M P
Limiting Elastic
Elastic- Plastic
Fully Plastic
Fig. 1.26. Stress distributions with increasing moment and curvature in an elastic-perfectly plastic material.
9
I
l
I
I
I
I
I
I
I
t
I
Mp
l
1/R
I
Curvature
E't
A (l/R)
Fig. 1.27. The moment-curvature diagram for an elastic-perfectly plastic sheet.
Unloading the plastic moment from mp to zero is associated with a change in bend angle A0 and a change in radius AR (fig. 1.28); the length of the neutral axis will remain unchanged, hence
(A(1/R)/(1/R)) + (A0/0) = 0
(1.29)
Combining (1.28) and (1.29), we can obtain the change in bend angle or spring-back as
AO = 3(S/E') (R/t)O
(1.30)
Equation (1.30) shows that the spring-back angle is proportional to the ratio of yield stress to elastic modulus. For annealed sheet, this is typically around 1 to 1,000; however, for hard temper sheet it may increase to 1 in 300 or greater. Equation (1.30) also shows that spring-back is proportional to the ratio of radius to sheet thickness. For small radius bends, such as are typical in roll forming, this may be around 2. For large radius bending, such as may be typical with autobody panels, this may be much higher, and spring-back will be large. Because of the variability in S, tl~e process may
22
J.L. Duncan and S.M. Panton
,
.... 9 --~~"-':~;i~::..'-.',.:m. ~ ~ i ~ : ~ . . , , ~.~i~ii:.'.'~..~..~ i ~ ~ "~'~:~!~....
! 9
,r3,
/
i i i
/
/ R 0
/
/
/
/
/ /
/
/
/
R+Z~R
Fig. 1.28. Spring-back of a sheet upon unloading of a moment. be difficult to control. A technique for avoiding these problems is discussed in the next section. If the unloading process from a fully plastic moment is elastic, there will be a residual stress distribution in the sheet, as shown in fig. 1.29. This is an idealised representation, but sheet metal that has been subjected to various bending, unbending and straightening processes is liable to have significantly more complex residual stress distributions. 1.6.2 9 Bending under tension
Equation (1.30) indicates that if a sheet is given a gentle curvature by the application of a moment, the spring-back would be large. To obtain accurate shape as, for example, in curving an exterior panel for an aircraft, the sheet is curved by stretching over a former, as shown in fig. 1.30. It will be seen from the stress distributions shown in fig. 1.30, that as the tension increases, the m o m e n t required to maintain a curvature less than the limiting elastic curvature will remain constant until the outer fibre stress reaches the yield stress S. When the tension has reached that required to stretch the sheet plastically, i.e.
Fig. 1.29. Residual stresses upon unloading.
Introduction to sheet metal forming
(a)
23
t
M
M
(b) (i)
S
(u)
......
(Iv) ~
S
(c) M Me
w
~9
T
St Fig. 1.30. (a) Bending under tension. (b) Stress distribution under increasing tension. (c) Moment required to maintain the curvature as the strip tension increases.
T - S t , the moment has reduced to zero and the spring-back due to bending will also be zero. In practice, the sheet will be stretched plastically by a few per cent and will then take up the radius of the former accurately.
1.7. Superplasticity The characteristic behaviour of metals and their alloys is that at room temperature they can be deformed plastically and will strengthen or work harden as they do so. The resistance to flow depends largely on the amount of deformation imposed and not on the rate of working. At higher temperatures, such as those used in hot forging, their strength will diminish and remain constant during deformation; they do not strain harden, but the flow strength is dependent on the rate of working. As the temperature increases, metals typically have a well-defined melting point and change from a solid with an appreciable, but still low, rate-sensitivity to a low-
J.L. Duncan and S.M. Panton
24
viscosity liquid. They do not display the semi-fluid highly viscous behaviour of materials such as glass or thermoplastics at the temperatures used for glass-blowing and blow-moulding. The ability to draw out a thin filament of glass from a molten pool or to blow a tube of molten polyethylene out to many times its diameter can be shown to depend on the fact that the resistance to flow is very nearly proportional to the rate of extension, i.e. these materials behave as ideal viscous liquids and imperfections do not become catastrophic. Although highly viscous behaviour is not a characteristic of metals, even at elevated temperatures, certain alloys do show moderate viscosities under unusual conditions. This phenomenon has been termed superplasticity. There are a few alloys which can be produced in a very fine grain condition, less than 10 microns, and this state is stable at temperatures up to about half of their absolute melting temperature. If these alloys are hot worked, they do not strain harden, but have a flow stress which obeys a law of the kind, O- - - B ~ m
where m, the strain-rate sensitivity index, is in the range 0.3 ~ 0.8. The alloys that have received most attention are Zn 22%A1 which is formed at 250~ and Ti 6%A1 4%V which is superplastic between 900 and 980~ If these materials are deformed in an elevated temperature tensile test, extensions of several hundred per cent are possible. The flow stress at these temperatures is low compared with typical hot-working strengths in metals but it is still higher than those observed in thermoplastics in moulding and blow-forming. Vacuum-forming can be used, but for reasonable production times, pressure forming is necessary. In designing superplastic forming processes, it is necessary to keep the strain rate within the range at which the rate-sensitivity index is highest; this may only extend over about a decade in the vicinity of 10 -3 s -1 . A useful example is illustrated in fig. 1.31 which shows the two-dimensional pressure forming of a sheet into a corner. If the sheet is clamped at A and B, the first stage of the process can be considered as uniform stretching of the sheet until it just touched the side-walls of the die; assuming incompressibility, the thickness at this instant is
A / / /
//////7-//t3
/ /
Fig. 1 . 3 1 . 2 - D p r e s s u r e f o r m i n g of a sheet into a c o m e r .
Introduction to sheet metalforming
25
tA -- (2~/2/:r)to F r o m this point onwards, the sheet is often assumed to stick to the die wall without further thinning and the current thickness, t, of the unsupported sheet tangent at the height, h, can be calculated by geometry. If the strain rate prescribed for the process is k0, the membrane stress is cr = p h / t and the required pressure is p -
tB ' /h
If it is desired to form into a small corner radius, the final value of h is small and the pressure could be high. As indicated, this usually precludes vacuum-forming. In the above analysis, the thickness is determined by geometry and diffuse necking is neglected. This is often an acceptable approximation in analysing superplastic process; however, it becomes less valid as the strain-rate sensitivity index decreases; more elaborate calculation may then be necessary.
References
[1] Hosford, W.F. & Caddell, R.M., Metal Forming: Mechanics and Metallurgy, Prentice Hall, New Jersey (1983). [2] Hill, R., The Mathematical Theory of Plasticity, Oxford University Press, London (1950), p235. [3] Marciniak, Z. & Kuczynski, K., Int. Journ. Mech. Sci., 9 (1967), p609. [4] Marciniak, Z. & Duncan, J.L., Mechanics of Sheet Metal Forming, Edward Arnold, London (1992).
This . Page Intentionally Left Blank
Composite Sheet Forming edited by D. Bhattacharyya 9 Elsevier Science B.V. All rights reserved.
Chapter 2
Thermoplastic Composite Sheet Form&g: Materials and Manufactur&g Techniques B. T o m a s , ~ S T R O M
Department of Aeronautics, Division of Lightweight Structures, Royal Institute of Technology, S-IO0 44 Stockholm, Sweden
Contents Abstract 28 2.1. Introduction 28 2.2. Constituents 29 2.2.1. Matrices 29 2.2.1.1. Polymer morphology 30 2.2.1.2. Structural aspects influencing properties 31 2.2.1.3. Thermoplastic polymer matrices 34 2.2.2. Reinforcements 38 2.2.2.1. Glass fibers 39 2.2.2.2. Carbon fibers 40 2.2.2.3. Organic fibers 41 2.2.2.4. Other fibers 42 2.2.2.5. Reinforcement-matrix interaction 42 2.2.3. Preimpregnated reinforcements 43 2.2.3.1. Solvent impregnation 44 2.2.3.2. Melt impregnation 45 2.2.3.3. Powder impregnation 46 2.2.3.4. Commingling 47 2.2.3.5. Comparison of preimpregnated reinforcement types 47 2.2.3.6. Molding compounds 48 2.3. Properties 48 2.3.1. Matrices 48 2.3.1.1. Thermal and rheological properties 49 2.3.1.2. Mechanical properties 52 2.3.2. Reinforcements 54 2.3.2.1. Thermal properties 54 2.3.2.2. Mechanical properties 54 2.3.3. Composites 55 2.3.3.1. Prediction of thermal properties 55 2.3.3.2. Prediction of mechanical properties 56 2.3.3.3. Experimentally determined thermal properties 57 2.3.3.4. Experimentally determined mechanical properties 58 27
28
B.T. flstrd'm
2.4. Manufacturing techniques 60 2.4.1. Prepreg lay-up 61 2.4.2. Prepreg consolidation 61 2.4.2.1. Vacuum-bagconsolidation 61 2.4.2.2. Matched-die consolidation 62 2.4.2.3. Double-belt-press consolidation 63 2.4.2.4. Tape laying 64 2.4.2.5. Intermittent matched-die consolidation 65 2.4.3. Sheet forming 65 2.4.3.1. Matched-die molding 66 2.4.3.2. Rubber-die molding 67 2.4.3.3. Hydroforming 68 2.4.3.4. Deep drawing 68 2.4.3.5. Diaphragm forming 69 2.4.3.6. Folding 70 2.4.3.7. Roll forming 70 2.4.3.8. Matched-die molding of GMT 71 Acknowledgement 72 References 72
Abstract
This chapter provides an introduction to thermoplastic composite sheet forming and the raw materials commonly used. First the relevant basics of polymer physics are introduced in order to provide a rudimentary background to the matrices' macroscopic properties and processing requirements, whereupon different reinforcement types and preimpregnated reinforcement forms are introduced. Second the thermal, rheological, and mechanical properties of common sheet forming raw materials and their composites are discussed and representative properties given. Finally a comprehensive yet brief overview of different composite sheet forming techniques, including blank consolidation processes, is presented. 2.1. Introduction
On the face of it, many structurally capable composites are shell-like components that one way or another ought to be manufacturable through conformation of a flat raw material blank into a complex-shaped final component. It should therefore come as no surprise that the topic of thermoplastic composite sheet forming is one of intense research, which has resulted in a number of forming techniques. Since the concept of thermoplastic composite sheet forming forming of a flat piece of material into an arbitrarily curved c o m p o n e n t - is identical to sheet metal forming, a few of the techniques investigated have been borrowed from this relatively mature manufacturing field, while others emanate from thermoset composites manufacture. Only a minority of the techniques discussed herein have genuinely been invented or developed exclusively for sheet forming of thermoplastic composites. While all forming techniques discussed in this chapter have proven technically feasible, widespread commercial success is rare. However, given the significant research and development
Thermoplastic composite sheetforming
29
efforts thermoplastic composite sheet forming is seeing, there should be little doubt that all this work gradually will lead to commercial successes in the near future. This chapter aims to give the novice to the topic of thermoplastic composite sheet forming an introduction to the raw materials used, their properties, and common forming techniques. The first two sections of the chapter introduce the constituents most commonly used and then go on to discuss the thermal and rheological properties so relevant to manufacturing. Since sheet-formed components are most likely to be used in structural applications, the mechanical properties of both constituents and their composites are also briefly treated. The final section of the chapter presents a comprehensive overview of sheet consolidation and sheet forming techniques, but since several of these techniques will be more thoroughly treated in other chapters of this volume this treatment is brief.
2.2. Constituents
The constituent materials that make up, or constitute, a composite are normally considered to include at least the matrix and the reinforcement. Oftentimes the matrix is not homogeneous but rather mixed with some performance-enhancing additive. Likewise, the reinforcement is normally surface treated or coated with some performance-enhancing substance. These substances may or may not be considered constituents on their own right. This section of the chapter covers the constituents most relevant to thermoplastic sheet forming and describes available types and family characteristics.
2.2.1. Matrices
The matrix of a composite has several functions: it is a binder that holds the reinforcement in place, it transfers external loads to the reinforcement, and it protects the reinforcement from environmental exposure. Moreover, the matrix redistributes the load to surrounding fibers when a fiber fractures and supports the fibers to prevent buckling in compression. Polymer matrices clearly dominate in composites applications, although other matrices are used to a limited degree in specialized applications; these other matrix types are not covered in this chapter. To fully appreciate differences between candidate polymer matrices in terms of properties and processing requirements, it is essential to at least have a conceptual understanding of polymer physics and chemistry. However, this treatment is primarily intended for readers with little chemistry background and the following sections therefore refrain from delving too far into the field of polymer science; the interested reader is referred to the literature specializing in this topic. The following treatment thus merely aims to provide a basic understanding of the polymerscience aspects most relevant to composites properties and their manufacturing requirements, and in particular matrices and issues pertaining to thermoplastic sheet forming.
B.T. ~lstrO'm
30
2.2.1.1. Polymer morphology A polymer is a high-molecular-weight compound that is composed of a multitude (poly) of repeated small segments (mers). Polymers are organic compounds primarily based on carbon and hydrogen atoms bound to each other by primary, or covalent, bonds. Carbon is capable of forming four covalent bonds located tetrahedrally around the atom. Carbon atoms may form covalent bonds to each other both through single and double bonds, the former being referred to as saturated and the latter unsaturated. (Carbon atoms can also bond to each other through triple bonds, but such bonds are seldom encountered in polymer science.) In contrast, hydrogen can form one covalent bond only. The least complex polymers are the hydrocarbon polymers which contain carbon and hydrogen only. The simplest hydrocarbon polymer is polyethylene (PE), the repeating unit of which is illustrated in fig. 2.1, where "n" indicates a large number (103-106) of repeating mers to form a practically useful polymer and " - - " indicates covalent bonds. It is important to note that the two-dimensional rendition of the structure in the figure in reality is three-dimensional due to the tetrahedrally arranged bonds of the carbon atoms. Another important and common hydrocarbon polymer is polypropylene (PP); see fig. 2.2. Several other hydrocarbon polymers besides PE and PP exist, although they are rarely of interest in composites applications. However, if one includes other elements than carbon and hydrogen, virtually endless combination possibilities arise. Apart from carbon and hydrogen, the most common elements are oxygen, nitrogen, sulfur, fluorine, chlorine, and silicon. As long as only carbon makes up the polymer backbone, one talks of carbon-chain polymers, whereas polymers having some non-carbon backbone atoms are referred to as heterochain polymers.
H
H
I
I
-(- C-- C-)-n I
H
I
H
Fig. 2.1. Repeating unit of PE. H
H
H
H
I
I
I
I
-(-- C - C-)-n I
H H-C-H
-(.- C-- C-)- n I
H
I
CH 3
I
H Fig. 2.2. Two ways of illustrating the repeating unit of PP.
Thermoplastic composite sheetforming
31
2.2.1.2. Structural aspects influencing properties There are strong relationships between the molecular structure, or configuration, of a polymer and its macroscopic properties in both solid and liquid form. These relationships may be hierarchically divided into intramer, intramolecular, and intermolecular structure. The next three subsections describe some molecular aspects of relevance and their influence on the polymer's macroscopic properties. Intramer structure. The properties of the polymer are to a large degree influenced by the structure of the mer, i.e. what elements are present and how they are bound to one another. Single bonds allow rotation around the bond axis (torsion), while double bonds do not. Double bonds and cyclic structures, such as the common aromatic ring (see fig. 2.3), in the backbone and large side groups leave the molecule inflexible and bulky, thus impeding molecular motion which significantly influences macroscopic properties. Polyisoprene is a good example to illustrate the strong influence of apparently subtle differences in mer configuration (see fig. 2.4); cis-polyisoprene (natural rubber) is soft whereas trans-polyisoprene (gutta percha) is a hard plastic. Note that these two mer configurations are different since the double bond does not allow rotation. The cis-prefix denotes that the backbone continues on the same side of the double bond and the trans-prefix that the backbone extends on different sides, cisPolyisoprene and trans-polyisoprene are said to be geometric isomers. Intramolecular structure. While the mer may be fully defined, there are still many combinations in which it may form a polymer. Taking PP as an example, the methyl (CH3) group may be located in different positions; see fig. 2.5. Isotactic PP has all methyl groups on the same side, syndiotactic on alternating sides, and atactic in a random manner. Even though single bonds permit rotation, these three forms of PP are different (recall the tetrahedral arrangement of the four bonds of the carbon atom). The regular structures of isotactic and syndiotactic PP, which are referred to
_ cIC'~c -C
I
II
O#
C-
I
Fig. 2.3. Two ways of illustrating the repeating unit of an aromatic group.
H I
H-C-H I
C I
-C-H I
H
H H I
C I
H-C-
I
H
I
H-G-H I
H I
H-GI
C
C
-C-H
H
I
I
I
H
Fig. 2.4. Repeating unit of c/s-polyisoprene (left) and trans-polyisoprene (right).
B.T. ~tstrO'm
32 H I
-CI
H
H I
H I
H I
H I
H I
C -C - C -C-
C-
CH3H
CH3
I
I
I
I
CH3H
I
H
CH3H
H
-C-
H
C -C-
C -C-
C-
H
CH3H
H
CH 3
I I
H I I
I
I
I
I
I
I
H
I
I
H
CH3H
H
-C-
C -C-
C -C-
H
CH3H
I
I
H
I
I
I
I
H
I I
H I
I
H I CI
CH3
Fig. 2.5. Isotactic (left), syndiotactic (center), and atactic PP (right).
as stereoisomers, translate into quite different macroscopic properties from those of atactic PP. Of great significance to the macroscopic properties of a polymer is the number of repeat units or, alternatively, the molecular weight. However, there is no way of producing polymers of a single molecular weight and in reality it may vary by three to four orders of magnitude within the same sample. While all polymer examples so far discussed have been linear with small side groups only, branching may occur. Further, no attention has been paid to the ends of the molecules, which obviously must deviate from the idealized polymer structure, but since the number of repeating units is so large possible effects of the end groups are most often ignored. The molecules may also contain impurities, i.e. some flaw inconsistent with the idealized polymer structure. To improve certain properties of a polymer it is possible to polymerize it from more than one type of monomer. Two different repeating units (here denoted A and B) thus may be polymerized into alternating (ABABABABABA), block (AAABBBBBBAA), random (ABBABAABBBA), or graft fashions, where the latter has a backbone made up entirely of one mer with branches made up entirely of the other one attached. Intermolecular structure. The interaction between molecules is a function of intramer and intramolecular structure. It was earlier pointed out that the intramolecular bonds are covalent. There are also secondary bonds, e.g. van der Waals, hydrogen, and dipole-dipole bonds, which act between molecules. The reason for referring to them as secondary bonds is that they are an order of magnitude weaker than the covalent bonds and therefore are of secondary albeit s i g n i f i c a n t - importance. At a sufficiently high temperature a polymer sample melts; the individual molecules of the melt are randomly arranged, interlaced, and undergoing constant rearrangement. The covalent bonds ensure the integrity of the molecules while the molecular movement caused by the heating dwarfs the secondary bond forces. If the polymer sample then very quickly is cooled, or quenched, into a solid the random molecular arrangement is essentially frozen in place by secondary bonds. However, if the polymer sample is instead cooled slowly, the individual molecules may, under certain conditions, attempt to align themselves into a regular crystal formation. The crystal conformation is preferred since it represents the lowest possible energy state for the molecules. Due to the precise close-packing of the molecules in the crystal state, the crystal structure has higher density than the random molecule arrangement, which is usually referred to as amorphous or glassy. Further, since the crystal conformation is preferred due to the lower energy state, energy is released upon crystallization, i.e. it is an exothermal process.
Thermoplastic composite sheetforming
33
In reality it is not possible to achieve complete crystallinity and amorphous areas therefore partly surround the crystals; polymers possessing the ability to crystallize are consequently referred to as semicrystalline. The degree to which a polymer may crystallize is to a large degree dependent on the molecule being regular in structure and flexible. This is the reason why isotactic and syndiotactic PP may form crystals whereas atactic PP may not, and why PE, due to its extremely simple, regular, and flexible structure, may achieve the highest degree of crystallinity of any polymer. Likewise, molecules that do not contain double bonds and cyclic structures in the backbone or bulky side groups are more likely to achieve a greater degree of crystallinity than if they had these features. Although many polymers of relevance for use as composite matrices are semicrystalline, most polymers are unable to achieve any appreciable degree of crystallinity under any circumstances. The resulting degree of crystallinity in a semicrystalline polymer is enhanced by higher temperature and pressure during crystallization as well as by lower molecular weight. From a manufacturing point of view, especially the former two dependencies are highly relevant. The temperature dependency of the degree of crystallinity is usually assessed in terms of cooling rate; see fig. 2.6. As the figure shows, it is possible to obtain either a more or less entirely amorphous structure through quenching of the melt or a highly crystalline structure through very slow cooling. Upon gradual heating of a semicrystalline polymer the amorphous regions melt before the crystalline regions and a melt with the random molecular arrangement is regained. The melting of the crystalline phase consumes energy in order to dislodge the molecules from their preferred low-energy state and the process is therefore endothermal. The reason why it is possible to reversibly go from solid to melt to solid etc. is that only secondary bonds act between molecules. A polymer with such a reversible behavior is called thermoplastic. In theory the melting and solidification cycles can be repeated an infinite number of times without affecting the polymer. In reality parts of some molecules will react chemically, i.e. covalent bonds will be destroyed or
50 40-
._r m m
L)
3020 10 0
~ 10 o
~ 101
~ 102
~ .... 103
C o o l i n g Rate [~
Fig. 2.6. Crystallinity of polyetheretherketone (PEEK) matrix in carbon/PEEK composite as function of cooling rate. Note the logarithmic cooling rate scale. Redrawn from reference [1].
34
B.T. flstr6"m
created, and the polymer and thus its properties will eventually degrade through oxidation, chain scission, etc. Under certain conditions covalent bonds may form between molecules. One of the more notable locations that readily become sites of such crosslinks is the unsaturated carbon-carbon double bond in the polymer backbone, which through a chemical reaction may open up, leaving a (saturated) single covalent bond within the molecule and creating new covalent bonds to other molecules. Starting from a polymer liquid consisting of molecules capable of forming crosslinks, any of a number of means may be employed to set off a chemical reaction which creates covalent crosslinks to neighboring molecules, thus creating a gigantic three-dimensional molecule. As crosslinks are formed the polymer liquid gradually loses its ability to flow since the molecules no longer can slip past one another as in the thermoplastic melt. The three-dimensional network translates into a lower energy state than the random molecular orientation of the liquid state, so the crosslinking process is (just like crystallization) exothermal. Since the three-dimensional network created is bound together by covalent bonds (in contrast to the previously mentioned intermolecular secondary bonds) it may not be melted through reheating. The type of polymer having the ability to crosslink is called thermoset. In conclusion there are two very different polymer f a m i l i e s - thermoplastics and thermosets. Thermoplastics consist of long molecules with only secondary bonds in between molecules and therefore may be melted. If irregular in structure and stiff, the molecules of a thermoplastic are randomly arranged both in the melt and in the solid; the polymer is amorphous. On the other hand, if the molecules are regular in structure and flexible, the molecules, while randomly arranged in the melt, may form crystals as the thermoplastic solidifies; the polymer is semicrystalline. However, the degree of crystallinity of a semicrystalline polymer is dependent on cooling rate; with a high cooling rate the solid polymer ends up more or less amorphous, whereas with a low rate it will be partly crystalline and partly amorphous, i.e. semicrystalline. Initially thermosets also consist of long molecules with only secondary bonds between them. However, under certain conditions, such as the presence of carboncarbon double bonds in the molecular backbone and chemically reactive substances in the bulk resin, covalent bonds may form between molecules, resulting in solidification of the resin. Since the intermolecular covalent bonds cannot be broken without simultaneously breaking the intramolecular covalent bonds, thermosets cannot be melted. As the molecular arrangement in solid thermosets (as well as in the liquid state) is random, thermosets are amorphous. While thermosets may be regarded as a special case in polymer science, it is a very important special case and thermosets clearly dominate over thermoplastics in virtually all composites applications. However, since the main topic of this volume is thermoplastic sheet forming, thermoset polymers will only briefly be mentioned in the remainder of this chapter.
2.2.1.3. Thermoplasticpolymer matrices While there is a vast array of engineering plastics available, only a few are used as composite matrices, since an engineering plastic with excellent properties does not necessarily make an excellent composite matrix. Issues that are of importance when
Thermoplastic composite sheetforming
35
selecting a polymer for use as composite matrix are reinforcement-matrix compatibility in terms of bonding, mechanical properties, thermal properties, cost, etc., though perhaps the most important aspect may be its processability, i.e. how easy is it to deal with it in manufacturing situations. Among the many issues that may be considered part of the processability are viscosity, processing temperature, processing time, and health concerns. The viscosity is important in achieving reinforcement impregnation, where each reinforcing fiber ideally should be surrounded by the matrix without voids present; impregnation is naturally facilitated by a low viscosity. Not-yet-crosslinked thermosets have shear viscosities at processing temperature of the order of 10~ Pa s, while melt viscosities of thermoplastics at processing temperature are of the order of 102 Pa s or higher (for comparison, the shear viscosity of water at room temperature is 10-3 Pa s), meaning that it is much easier to complete impregnation with thermosets than with thermoplastics. Once impregnation is completed, thermoplastics only need to be melted, shaped, and then cooled to achieve dimensional stability in a matter of seconds, although the temperatures required can be quite high by polymer processing standards. In contrast, thermosets need several minutes to several days for crosslinking to be completed, albeit normally at lower processing temperatures than with thermoplastics. The chemical structure of thermoplastics makes them chemically inert if processed correctly, meaning that no hazardous byproducts need to be considered. On the other hand, the molten thermoplastic and the heated machinery may cause severe burns. This relative lack of health worries is a distinct advantage over thermosets which, due to the active chemistry, give rise to considerable health concerns. A thermoplastic is usually fully polymerized when delivered from the supplier, meaning that all chemical reactions are completed and the user can concentrate entirely on physical processes, such as heat transfer and flow. However, there are some rare exceptions to this rule. The user may choose to take care of part of the polymerization starting off with low-molecular-weight prepolymer, thus avoiding the high-viscosity disadvantage during reinforcement impregnation. Courtesy of the low molecular weight, the polymer fluid may have a viscosity comparable to that of a thermoset resin. After the reinforcement is impregnated, the final polymerization process takes place and the molecular weight thus drastically increases. Depending on the type of polymer, the high-molecular-weight polymer may or may not decompose into lower-molecular-weight polymer molecules upon remelting. One of the main features of amorphous thermoplastics is that they are dissolvable in common industrial solvents. This means that the reinforcement can be impregnated with a low-viscosity solution, thus avoiding the problem of high melt viscosity, but it also means that the solidified polymer (and composite) is not solvent-resistant. For solvent-impregnated reinforcement, the residue solvent that was not completely driven off after impregnation is a serious concern since it impairs the quality of the composite. Amorphous thermoplastics do not shrink much when they solidify, which translates into good surface finish. Semicrystalline polymers usually have good solvent-resistance due to the crystallinity which prevents dissolution of the entire molecular structure. The crystallinity also improves high-temperature performance and long-term phenomena, such as
36
B.T. AstrO'm
creep. If the crystallinity is too low, these benefits are not seen and if it is too high the material loses toughness and becomes brittle, although it usually gains in stiffness. Hence, there is an optimum degree of crystallinity. When processing semicrystalline polymers one thus must consider, and preferably control, the cooling rate (see fig. 2.6), which rarely is an issue with amorphous matrices. Useful semicrystalline polymers have 5 to 50 volume percent crystallinity, with an optimum of 20 to 35 percent for composites applications [2]. Semicrystalline polymers shrink more than amorphous ones upon solidification; the higher the final crystallinity, the higher the density change between melt and solid. Due to the difference in shrinkage between the amorphous and the crystalline regions, the surface of semicrystalline thermoplastics is generally not as good as for amorphous ones. Since solvents normally cannot be used to dissolve semicrystalline polymers (there are some rare exceptions), reinforcement impregnation is extremely difficult. The following subsections aim to give a brief overview of some of the more common thermoplastic polymers used as composite matrices; table 2.1 shows their respective repeating units. The characteristics discussed below are merely family characteristics and large variations are the rule. Polyethylenes. PE can be both commodity (not intended for structural applications) and engineering plastic depending on grade, but is rarely used as composite matrix due to low temperature tolerance and low mechanical properties. However, PE fibers may be used as composite reinforcement. PE has the highest degree of crystallinity of any polymer due to its simple, regular, and flexible molecular structure. Polypropylenes. Just like PE, PP is both commodity and engineering plastic depending on grade. PP is the chemically least complex and cheapest polymer commonly used as composite matrix. In structural composites applications PP is usually reinforced with glass fibers. In recent years PP has become the most common thermoplastic matrix in mass-produced structural composites applications, including automobile components, such as various engine-room parts and seatback frames. Polyamides. One of the best-known thermoplastic polymer families is the polyamides (PA). While Nylon originally was the (Du Pont) trade name for PA fibers, "nylon" (not capitalized) gradually has become an accepted designation for PAs regardless of manufacturer. In contrast to PE and PP, PAs may be used at moderately increased temperatures thus greatly improving its usefulness as matrix. PAs are categorized by the presence of amine groups (--CONHm). A number of different PA grades, e.g. PA 6, PA 6,6, PA 6,10, and PA 12, are available, where the numbers indicate the number of carbon atoms in the repeating unit (see table 2.1); the properties naturally vary accordingly. The biggest drawback of PAs is that they are hygroscopic, i.e. absorb water. In composites applications PAs are normally reinforced with glass fibers and used in applications similar to glass/PP, but where higher temperature tolerance and improved mechanical properties are required. Thermoplastic polyesters. Although perhaps chiefly recognized as thermoset resins, polyesters also are available in thermoplastic forms, e.g. poly(ethylene terephthalate) (PET) and poly(butylene terephthalate) (PBT). The properties of
Thermoplastic composite sheet forming
TABLE
37
2.1
Comparison
of thermoplastic
Polymer
candidates for composites
Mer Structure H
Polyethylene, PE
H
I I~ ~CmC I HI H H
Polypropylene, PP
H
I I mC~C~ I I H
CH 3
0 Polyamide 6, PA 6
H
II C
Polyamide 12, PA 12
(CH2) 5~
~
H
II
I
H
H
0
I
I
II
~N~
Poly(phenylene sulfide), PPS
I
N
0
Polyamide 6,6, PA 6,6
Poly(ethylene terephthalate), PET
applications
(CH2)6~N~
O~
(CH2)2~ O~
C~
0 (CH2)4~
II
C~
O
O
[C[
C
-~s_
_~~_~o_~o_ o
Poly(ether ether ketone) PEEK
o Poly(ether sulfone), PES
II
o
o
o
II
/c~~.~
Poly(ether imide), PEI
CH,
_N,~~.~o_~ i~_~ o_~ :~_~ ,,
O
O O
II
Poly(amide imide), PAI
II
c
_~ ~_~o_~ II
o
38
B.T. ~lstr6"m
PET and PBT are similar to those of PAs, but lacking the hygroscopic disadvantage. In composites applications thermoplastic polyesters are reinforced with glass fibers and used in applications similar to glass/PP and glass/PA. Poly(phenylene sulfides). The most common member of the poly(arylene sulfide) family is poly(phenylene sulfide) (PPS), which has good tolerance to most chemicals and fire. PPS exhibits intermediate mechanical properties and temperature-tolerance. In composites applications PPS is reinforced with glass or carbon fibers and used in high-performance applications. Polyketones. While there are numerous aromatic polyketones, such as poly(ether ketone) (PEK), poly(ether ketone ketone) (PEKK), etc., the most common is poly(ether ether ketone) (PEEK). The polyketones possess high mechanical properties, high temperature-tolerance, good solvent resistance, and a high price. In composites applications PEEK is reinforced with glass or carbon fibers and used in critical high-performance applications. Polysulfones. Polysulfone (PSU), poly(ether sulfone) (PES), and poly(aryl sulfone) (PAS) are high-performance amorphous polymers with good tolerance to high temperatures and fire. These properties naturally come at a high cost and the melt viscosities are very high. Since polysulfones are amorphous, they are not resistant to all solvents although their resistance to many chemicals nevertheless is very good. In composites applications polysulfones are reinforced with glass or carbon fibers and used in critical high-performance applications. Thermoplastic polyimides. The polyimide family includes poly(ether imide) (PEI), polyimide (PI), and poly(amide imide) (PAI), which are all amorphous. Polyimides have the highest temperature-tolerance of the thermoplastics mentioned herein. Despite being amorphous they are very tolerant to solvents and environmental exposure and offer very good mechanical properties with the disadvantages of very high viscosities and high cost. In composites applications the members of the polyimide family are reinforced with glass or carbon fibers and used in critical highperformance applications.
2.2.2. Reinforcements The reinforcement is the constituent that is primarily intended to carry the structural loads the composite is subjected to. The reinforcement therefore to a significant degree determines stiffness and strength of the composite as well as several other properties. Composite reinforcement may be of different forms, but only fibrous reinforcement is relevant to thermoplastic sheet forming. A fiber, or filament, has a length-to-diameter ratio that approaches infinity and a diameter of the order of 10-5 m. All common fibers are manufactured in a drawing process, where the liquid raw material is drawn from an orifice. The drawing process ensures that the molecules of fibers organic in origin are aligned and parallel to the drawing direction, translating into significantly higher strength and stiffness in the axial direction than transverse to it. The most common types of fibrous reinforcement used in composites applications are glass, carbon, and aramid. However, it is not only the fiber type that
Thermoplastic composite sheet forming
39
is of significance; equally important is its configuration or form, e.g. the fibers may be discontinuous or continuous, randomly arranged or oriented, all aligned or in fabric form, etc.
2.2.2.1. Glass fibers The major ingredient of glass fibers is silica (SiO2), which is mixed with varying degrees of other oxides. The mixture is melted and extruded through minute holes in a platinum-alloy plate, or bushing. The glass filaments (fibers) vertically emerging from the bushing are drawn at high speed and are then quenched by air or water spray to achieve an amorphous structure. A protective coating is applied to the filaments before they are gathered together and wound onto forming packages. The wet glass is then dried. A group of collimated glass fibers is called a tow, strand, or yarn and an assembly of collimated tows is called a roving. When the tows are wound onto forming packages, as well as when tows are joined into rovings, they are usually rotated to provide a so-called twist, which promotes integrity and thus simplifies subsequent handling, while at the same time making impregnation more difficult since it becomes more difficult to spread the fibers prior to impregnation. The diameter of the individual filaments varies between 5 and 24 ~tm and is in composites applications commonly in the range 10-20 ~tm. The size of glass tows and rovings is given by tex number (weight in grams of 1,000 m) or yield in yd/lb (in North America). Common tex numbers are 600, 1,200, 2,400, etc., while common yields are 900, 450, 225, etc. (1 yd/lb ~ 500,000/tex). Several different glass compositions are available, the most common being E and S glass, where "E" denotes electrical and "S" high strength. E glass offers excellent electrical properties and durability and is considered a general-purpose grade that heavily dominates consumption. S glass and R glass are similar and offer improved stiffness and strength as well as high-temperature tolerance. Not surprisingly, the latter glass types are considerably more expensive than E glass. ECR glass (_c.orrosion resistant) and C glass are similar and, while having properties similar to E glass, offer improved corrosion-resistance. Since there are several different glass compositions, there is naturally a large variation in properties. Nevertheless, characteristics that tend to be shared by all glass fiber types are: 9 Good mechanical properties 9 High temperature-tolerance 9 Positive coefficient of thermal expansion (CTE) 9 Good electrical properties 9 Good corrosion-resistance 9 Moisture-sensitive 9 Abrasive 9 Inexpensive A characteristic that sets glasses apart from other reinforcements used in composites applications is that they are amorphous (i.e. glassy) and therefore are isotropic.
40
B.T. ~lstr6"m
2.2.2.2. Carbon fibers
Carbon fibers are commercially manufactured from three different precursors: rayon, polyacrylonitrile (PAN), and petroleum pitch. In the first two cases, the starting point of the carbon-fiber manufacturing process is textile fibers, whereas fibers are spun directly from the melt when pitch is the starting point. The fibers are initially drawn and oxidized at temperatures below 400~ to crosslink them to ensure that they do not melt during subsequent processing steps; drawing and oxidizing may occur concurrently. The fibers are then carbonized above 800~ in a process called pyrolysis, i.e. in the absence of oxygen, to remove noncarbon elements and create fibers virtually consisting of carbon only. Graphitization is then carried out at temperatures above 1,000~ to further eliminate impurities and enhance crystallinity. During both carbonization and graphitization further drawing may be employed to enhance orientation within the fibers. After graphitization fibers are surface treated and size is applied. The carbon atoms are covalently bonded together in so-called graphene layers which are held together by secondary bonds. The properties of carbon fibers are the result of the strong covalent carbon-carbon bonds within the graphene layers and it is therefore mainly the degree of orientation of these layers that determines the properties of the fiber. A higher temperature during graphitization promotes orientation of the graphene layers in the fiber direction, thus resulting in a higher tensile modulus. Carbon fibers are supplied in tows denoted 3K, 6K, 12K, etc., depending on the number of individual filaments they contain, where for example 3K stands for 3,000 filaments. Carbon fiber tows receive little or no twist. Filament diameters vary between 4 and 11 ~tm and is commonly around 7 ~m. Carbon fibers are often quantitatively referred to as "ultra-high modulus", "high modulus", "intermediate-modulus", "high strength", etc., where the borders between categories gradually change due to the rapid development of new fiber types. Properties significantly depend on precursor type and heat treatments used. While carbon fibers have the highest strength and stiffness of any compositereinforcement candidate, they generally only provide high strength or high modulus (in the same fiber). The span in properties of different carbon fiber types is vast, but among the properties they tend to share (at temperatures relevant to polymer composites) are: 9 Outstanding mechanical properties 9 High temperature-tolerance 9 Negative longitudinal CTE, positive transverse CTE 9 Electrically conductive 9 Excellent environmental resistance 9 Insensitive to moisture 9 Brittle 9 Expensive to very expensive The negative longitudinal CTE is due to bending of the predominantly longitudinally aligned graphene layers, for which reason the negative CTE increases in numerical value as the modulus (and graphene layer orientation) increases. Whereas the con-
Thermoplastic composite sheetforming
41
ductivity of carbon may be advantageous in some cases it is often a disadvantage. Carbon fibers thus may cause galvanic corrosion of metallic inserts and loose carbon particles suspended in the air may easily short out electrical and electronic equipment. In manufacturing operations dealing with unimpregnated carbon fibers which may be abraded, it is therefore necessary to provide costly shielding of electrical and electronic equipment.
2.2.2.3. Organicfibers While several different organic fiber types have been used as composites reinforcement, the category is dominated by aramid fibers. Kevlar is often assumed synonymous with aramid, but is in fact just the (Du Pont) trade name of the most common of a few commercially available aramid fiber types. Aramids, short for aromatic polyamides, are members of the PA family; fig. 2.7 illustrates the repeating unit of Kevlar (cf. PAs, table 2.1). Aramid fibers are manufactured in a process called solution spinning. The polymer powder is dissolved in sulfuric acid and is extruded through small holes, or spinnerets, into a narrow air gap. The fibers are quenched in a water bath to solidify the fibers and wash off most of the acid. The fibers are further washed, dried under tension, and then wound onto spools. Since aramid fibers are not brittle a protective size is not necessary. When the polymer solution is extruded through the spinneret, the molecules align with the direction of shear and the subsequent quenching ensures that the orientation remains in the final fiber. The degree of orientation may be further enhanced by heat treatment under tension resulting in improvements in longitudinal modulus. Due to its high degree of crystallinity and rigid molecular structure the temperaturetolerance of aromatic polyamide is very good for an organic material. The fiber diameter is typically 12 lam and tows, which are not twisted, consist of anything from a couple of dozen to several thousand fibers per tow. Tows are normally designated either by the number of fibers or the denier count (weight in grams of 9,000 m). Characteristics of aramid fibers when used as composites reinforcement include: 9 Very good mechanical properties, especially toughness and damage tolerance 9 Moderate temperature-tolerance 9 Negative longitudinal CTE, positive transverse CTE 9 Good electrical properties 9 Fair corrosion-resistance 9 Very moisture-sensitive 9 Tough 9 Expensive
-C
0 I1_0~_
0 H II I _.0~_ C-N
Fig. 2.7. Repeating unit of Kevlar.
H I N-
42
B.T. ~lstrO'm
While possessing several attractive properties, aramid also gives rise to a few notable difficulties. From a design point of view it is important to realize that the strength in compression is only a fraction of that in tension and that the fiber-matrix compatibility generally is poor. The outstanding toughness of aramid creates a problem in that fibers are very difficult to cut and machining of aramid-reinforced composites therefore requires special tools and techniques. Polyethylene fibers. High-modulus PE fibers may be manufactured through a process called gel spinning, which is a variant of the solution spinning process used for aramids. Since the tensile properties of both PE and aramid fibers are dictated by the properties of the covalent bonds of the molecular backbones, their mechanical properties are similar, but due to the lower density of PE fibers their specific strength and modulus are higher and comparable to carbon-fiber properties. The main drawbacks of PE fibers are poor matrix compatibility and poor temperature-tolerance, which likely makes PE fibers impossible to use with thermoplastic matrices.
2.2.2.4. Other fibers Several specialty fibers are used in different applications, for example offering extra-high temperature-tolerance, radar transparency, etc. Fibrous reinforcements used in polymer-matrix composites applications include boron and ceramic fibers, metal wires, and natural fibers, such as jute and wood. None of these fiber types is common in sheet forming applications.
2.2.2.5. Reinforcement-matrix interaction Conceptually a fiber-reinforced composite consists of transversely isotropic fibers and isotropic matrix with a perfect bond in between. Reality, however, is significantly more complicated. For a composite to be able to support external loads, fibers and matrix must cooperate.'It is often assumed that the fiber-matrix bond should be perfect, i.e. have the same properties as the matrix, and as strong a bond as possible is indeed often desirable to improve, for example, interlaminar shear strength, delamination resistance, fatigue properties, corrosion-resistance, etc. However, in some load cases a weak bond actually may be preferable; damage tolerance of a composite with a brittle matrix is usually enhanced by a weak fiber-matrix bond [3]. Whatever the load case, the fiber-matrix interface is of crucial importance to the properties of a composite. Manufacturers of brittle fibers, such as glass and carbon, apply a size, or finish, to the fibers to protect them from damage during subsequent handling, such as spinning, weaving, etc. Since a single reinforcement roving may contain tens of thousands of fibers and thus may be difficult to handle, the size also may be intended to promote tow integrity during such handling. However, since a fiber coating may interfere with the creation of a strong interface, and promotion of tow integrity is detrimental to reinforcement impregnation, the size may be seen as a necessary evil. Consequently the size in some instances is removed, e.g. burned off, when subsequent handling has been completed. To enable application of the size to every fiber, it is in glass manufacture applied before the fibers have been gathered into a tow,
Thermoplastic compositesheetforming
43
whereas a carbon-fiber tow must be spread out as widely as possible before application. A good bond between fiber and matrix may be formed through several mechanisms that all require wetting of the fibers by the resin. The preferred bonding mechanism is chemical (covalent) bonding, whereas mechanical interlocking may work well if the fiber surface is irregular, which is the case with some carbon and organic fiber types. Assuming that the fiber is porous, interdiffusion of polymer molecules into the fibers offers another possibility, whereas electrostatic attraction (secondary bonds) probably does not offer a strong enough bond to alone be responsible for satisfactory bonding [4]. However, despite over thirty years of intense research, the true mechanisms behind most successful fiber-matrix bonds are not well understood. Moreover, successful recipes are jealously guarded trade secrets. For glass fibers a coupling agent is applied to the fiber surface to enhance fibermatrix compatibility. Well-functioning coupling agents are available for thermosets such as unsaturated polyesters and epoxies, whereas coupling agents for high-temperature thermosets and all thermoplastics are not as efficient or even nonexistent. However, much work is underway to develop coupling agents for thermoplastic matrices. For carbon fibers the situation is rather different in terms of achieving fiber-matrix compatibility. Instead of applying a coupling agent the fiber is treated so as to promote its reactivity and compatibility with the matrix. Most commonly the fiber surface is oxidized to create surface oxygen groups that can form covalent bonds with the matrix. It appears that mechanical interlocking also is important with carbon fibers, since bonding generally is less good for high modulus fibers which have a higher degree of orientation of the graphene layers and thus smoother surfaces. For organic fibers the situation is further different in that no size is needed to protect the tough fibers and that no successful coupling agent has been developed. A common misconception is that the properties of the matrix are uniform throughout the composite, but various studies have proved the existence of a matrix property gradient from the fiber surface into the matrix bulk, a so-called interphase region (not to be confused with the interface). Without such an interphase there would be a huge discontinuity in modulus at the fiber-matrix interface. It has proven to be advantageous to some properties to have an intermediate modulus or ductile interphase [4]. With some semicrystalline matrices the fibers act as nuclei for crystallization, meaning that the interphase may become highly crystalline and hence stiffer than the bulk matrix.
2.2.3. Preimpregnated reinforcements One of the most complex, difficult, and not least important aspects of composites manufacturing is the impregnation of the reinforcement, particularly if the matrix is highly viscous. Consider a carbon-fiber-reinforced composite with a fiber volume fraction of 0.6, an average fiber diameter of 7 ~tm, and a volume of 1 ml (a cube with 10-ram sides). This volume contains 16 km of fiber, 0.4 ml of matrix, and 0.34 m 2 of interface. If the matrix is a high-viscosity molten thermoplastic it is
44
B. T. ,4str6m
not difficult to imagine that it is extremely difficult to evenly spread 0.4 ml of matrix onto a fiber surface area equivalent to five and a half pages of normal writing paper. Invariably, the impregnation will be imperfect and result in some dry fibers and entrapped gas as well as nonuniform fiber distribution. This is the background to the widespread use of preimpregnated reinforcement (prepregs) in manufacturing of high-cost and high-performance composites. Commercial prepregs are manufactured with dedicated machinery under well-controlled conditions and the result is low void content and reasonably uniform fiber distribution, and the prepregs often contain matrices that are not for sale except in prepreg form. The significant convenience of prepregs naturally comes with a significant disadvantage in terms of high cost. Prepregs are available in several forms depending on reinforcement and matrix as well as intended use. With continuous and aligned reinforcement the major impregnation forms are solvent impregnation, melt impregnation, powder impregnation, and commingling. Preimpregnated discontinuous and randomly arranged reinforcement is common in compression and injection molding processes. Such molding compounds, which may be melt or powder impregnated, are not referred to as prepregs although they conceptually belong to the same category; they are further discussed in section 2.2.3.6.
2.2.3.1. Solvent impregnation
Recalling earlier sections of this chapter, amorphous thermoplastics are not resistant to all solvents and thus may be dissolved and used in solvent impregnation. The polymer is dissolved to significantly lower its viscosity and thus facilitate reinforcement wetting and impregnation. The reinforcement is led into a solvent bath where the combined efforts of surface tension and the fact that the reinforcement is guided over rollers or bars ensures impregnation. Emerging from the bath, the impregnated reinforcement goes through nip rollers that carefully meter the reinforcement-tosolution ratio, whereupon the impregnated reinforcement goes into a drying oven, where the solvent is driven off and recovered (see fig. 2.8). Thermoplastic prepregs are not sticky and no backing paper is used; rolled-up prepregs are stored at room temperature. Correctly performed solvent impregnation produces intimately impregnated reinforcement (see fig. 2.9a). Both rovings and fabrics may be impregnated in
Fig. 2.8. Schematic of solvent impregnation.
Thermoplastic composite sheetforming
45
Fig. 2.9. Cross-sections of different prepreg types. (a) Solvent- or melt-impregnated. (b) Powderimpregnated with polymer sleeve. (c) Commingled. Reinforcing fibers are black and matrix is gray. Matrix powder particles and fibers typicallyhave significantlylarger diameter than reinforcing fibers.
this fashion. Regardless of resin type, residue solvent in the matrix presents a problem since it may be seriously detrimental to the properties of the composite. 2.2.3.2. Melt impregnation Ideally, melt impregnation is the preferred impregnation process, since it completes the ultimately desired intimate fiber wetting without introduction of a solvent (see fig. 2.9a). Unfortunately it is also the most difficult impregnation technique due to the high viscosities involved; with thermoplastics the resin has the consistency of chewing gum. In this case surface tension is of little help, and the first impulse may be to somehow increase the transverse pressure to force the matrix into the reinforcement. However, an increased pressure also compacts the fiber bed further and thus makes it even less permeable, so this tactic has the opposite effect. Some melt-impregnation techniques for thermoplastics involve the application of molten matrix onto the reinforcement right before the nip between the spread-out reinforcement and a rotating roller. With this approach the pressure forces the matrix through the reinforcement towards the lower pressure on the other side of the reinforcement, i.e. along the direction of the negative pressure gradient. Following several rollers like these the process is finished off with nip rollers to ensure that the reinforcement-matrix ratio is correct. The newly fabricated prepregs are cooled by calendering rolls and the matrix solidified. Melt-impregnation techniques of this type, which are carefully guarded by patents, are probably only used to impregnate parallel-fiber tows or yarns, since attempts at impregnating fabrics likely would prove extremely difficult due to the restrictions of tow cross-overs. An alternative melt-impregnation technique capable of impregnating fabrics employs a double-belt press (DBP) (see fig. 2.10). A DBP essentially consists of
46
B.T. ~IstrO'm
Fig. 2.10. Schematic of double-belt-press prepregging of continuous fabric with thermoplastic matrix. two steel belts that feed the material through the machine while applying lateral pressure to the material. In the first section of the machine the steel belts are heated, while in the latter section the belts are cooled. A reinforcement fabric sandwiched between two polymer films is fed into the machine. The heat within the press melts the polymer films and a pressure gradient applied by the belts causes the molten polymer to impregnate the fabric, which finally is cooled before exiting the press. Since the residence time within the double-belt press is long, even highly viscous thermoplastics are capable of percolating the reinforcement structure. An interesting concept is offered by the thermoplastic long discontinuous-fiberreinforced (LDF) material. In this melt-impregnated prepreg product, the fibers are aligned as in an ordinary melt-impregnated prepreg, but the fibers are discontinuous, allowing forming not possible with continuous-fiberreinforced prepregs.
2.2.3.3. Powder impregnation By grinding the solid matrix into a fine powder, the reinforcement can be impregnated using a slurry or a fluidized powder bed. A slurry employs a liquid, often water, to disperse the powder and impregnate the reinforcement with the lowviscosity aqueous solution, whereupon the water is driven off. The slurry may contain some kind of agent to promote adhesion between matrix powder and fibers, or the powder-impregnated reinforcement may be pulled through an oven to slightly melt the powder onto to the fibers. A fluidized powder bed contains a powder cloud that is kept fluidized by circulating air. Correctly performed, electrostatic attraction and/or friction ensures that the reinforcement passing through the powder cloud is properly filled with resin particles. The use of an oven to fuse the matrix onto the fibers is common. Another option to prevent the powder from being shaken out of the reinforcement during subsequent handling involves enclosure of the powder-filled yarn in an extruded polymer sleeve of the matrix material (see fig. 2.9b). The main advantages of powder-impregnated reinforcements is that they are flexible (unless subsequently excessively melted) and that they are cheaper than solventand melt-impregnated prepregs. The main drawbacks are that the reinforcement is
Thermoplastic composite sheet forming
47
not completely melt-impregnated, which thus has to be undertaken during composite component manufacturing, and that the powder rarely is evenly dispersed within the reinforcement. The final melt impregnation is often difficult to satisfactorily achieve and the results are liable to be less good than if melt-impregnated prepregs had been used. Another drawback specific to slurry-impregnated materials is that they may suffer from residue adhesion agent translating into problems similar to those encountered with solvent-impregnated prepregs. Powder-impregnated reinforcement, which tends to be unidirectional, is rarely referred to as prepreg, but rather powder-impregnated tow or yarn. However, not only yarns but also fabrics may be powder-impregnated; resin powder is first distributed onto one side of the horizontal fabric and the powder thermally fused in place, whereupon the other side of the fabric receives the same treatment. Such a powder-impregnation process may be followed by a DBP to produce a fully melt-impregnated fabric.
2.2.3.4. Commingling Commingled reinforcement consists of mechanically commingled (combined) reinforcing fibers and fibers spun from a thermoplastic resin (see fig. 2.9c). The advantages and limitations of commingled prepregs are the same as for powderimpregnated yarns (with the difference that no worry of residues from a slurry impregnation is warranted). Commingled reinforcement is unidirectional and is usually referred to as commingled tow or yarn.
2.2.3.5. Comparison of preimpregnated reinforcement types A qualitative comparison of the products of the aforementioned impregnation methods would consider flexibility, quality of impregnation, and cost. Flexibility is highly desirable to allow conformation to curved shapes and to allow for use in textile processes. High quality of impregnation is of course always desirable and likewise cost should be kept as low as possible. In general solvent- and melt-impregnated prepregs possess limited flexibility. Not surprisingly, high quality of impregnation goes hand in hand with high cost in solvent- and melt-impregnated prepregs. The main advantages of powder-impregnated and commingled reinforcements is that they are flexible enough to be used in textile manufacturing processes such as weaving, braiding, etc. and that they are, on a relative scale, inexpensive. Their main drawback is that the reinforcement is not melt-impregnated, which creates processing difficulties at a later stage. (It deserves to be pointed out that also narrow tapes of solvent- and melt-impregnated prepregs may be used in very specialized weaving processes.) There are relatively few thermoplastic prepregs on the market; available combinations include glass-fiber-reinforced PP, PAs, thermoplastic polyesters, as well as carbon-fiber-reinforced high-performance thermoplastics. Fiber volume fractions of unidirectionally or fabric-reinforced thermoplastic prepregs normally range from 0.35 to 0.6.
48
B.T. flstr6"m
2.2.3.6. Molding compounds Many techniques to manufacture composites with more or less randomly oriented and often discontinuous reinforcement also use some form of preimpregnated reinforcement as raw material. However, when preimpregnated reinforcement does not contain oriented and essentially continuous fibers, it is usually not referred to as prepreg but rather as molding compound. With molding compounds it may be more appropriate to talk about reinforced resin rather than impregnated reinforcement, since the fiber content tends to be considerably lower than in prepregs. Glass-mat-reinforced thermoplastic (GMT) is available in sheet form reinforced with randomly oriented fibers, which may be discontinuous or continuous. The most common technique to manufacture GMT is to use a DBP (see fig. 2.10), where two random-fiber mats and three polymer films or layers of extruded molten polymer are sandwiched before entering the press. Since this type of more or less completely meltimpregnated GMT ends up being a few millimeters thick and thus stiff, it is usually stored fiat instead of being rolled up. In another technique to manufacture GMT, which is similar to paper-making, chopped fibers, resin powder, and additives are dispersed in a slurry, which is deposited onto a moving belt where the water is driven off. This type of GMT thus consists of a porous fiber structure containing matrix powder, which, if desired, may be more or less completely melt-impregnated in a DBP. GMT is also available with part of the reinforcement continuous and oriented; alternatively, randomly reinforced GMT may be combined with continuous-fiberreinforced prepregs right before molding. Fiber volume fractions are normally 0.1-0.3 and fiber lengths in the range 10-30 mm unless the reinforcement is continuous. The commercial incarnation of GMT is massively dominated by glass-reinforced PP. 2.3. Properties The emphasis of this section 2.3 is on properties relevant to manufacturing and basic mechanical properties and intentionally refrains from delving into the quagmire of mechanical properties such as impact, fracture, fatigue, creep, etc. The intention of this section is merely to give the reader a feeling for typical properties of constituent materials on their own and in composite form. The properties quoted herein are from several different sources and thus may be slightly contradictory, which illustrates the significant differences existing between material formulations, processing conditions, test methods, etc. Unless otherwise noted, all properties are for room-temperature (RT) conditions.
2.3.1. Matrices For a matrix to be able to perform its tasks of supporting and protecting the primarily load-bearing reinforcement a number of properties are of relevance. The most pertinent properties usually are moduli and strengths in tension, compression, and shear, while also ultimate strain and fracture toughness may be important. The
Thermoplastic composite sheetforming
49
properties of the matrix usually determines the environmental tolerance of a composite; tolerance to elevated temperature and aggressive environments, such as UV radiation, oxygen, solvents, water, etc., thus are of paramount importance. As with most property comparisons of such broad material families indeed, as with all quantitative information of this section 3 the information should be seen as indicative only.
2.3.1.1. Thermal and rheological properties At sufficiently low temperatures an amorphous polymer is a glassy solid and any macroscopic deformation is likely due to stretching of secondary bonds and angle deformation of covalent bonds and only involves segments consisting of a few atoms. As temperature increases a region of rapid loosening of the secondary bonds is encountered and significantly larger segments of the molecules become free to move through rotation of covalent bonds. The temperature where these changes take place is referred to as the glass-transition temperature, Tg (see fig. 2.11), and is accompanied by a decrease in stiffness of several orders of magnitude. As the temperature increases further, amorphous thermoplastics often have a so-called rubber plateau where the stiffness does not decrease significantly and deformations are due to molecules sliding past one another. Further heating leads to complete melting. Thermosets, on the other hand, which are always amorphous, tend to have an extended rubber plateau, but since covalent bonds hold the polymer network together the polymer never melts. (However, if the temperature increases enough, the polymer will start to degrade, i.e. covalent bonds will be broken or formed.) Semicrystalline thermoplastics also show a drop in stiffness at Tg since the amorphous regions lose so much stiffness (see fig. 2.11). However, the crystalline regions remain unaffected and act as physical crosslinks and the polymer keeps much of its macroscopic stiffness. Not until the crystalline melting point, Tin, is reached does the polymer completely melt from a macroscopic viewpoint. Since the transition temperatures (rig and Tin) are functions of the molecular mobility in the bulk polymer it is easy to appreciate that a more rigid molecular
lO,
"--" 102 ~ 101 ,
i
i
alline i ~~morphous
100 10-1
-~ rr 10.2 10-3 , 50
~ o w t T~100
_-~i 9 Cr~
L molecular\ weight \ 150
High i \ molecular \ weight i I --. ; T~ 250 200
Temperature [~
Fig. 2.11. Relaxation modulus of polystyrene (PS) as function of temperature. Note the logarithmic stiffness scale. Approximate positions of Tg and Tm added. Redrawn from reference [5].
B. T. .~str6"m
50
structure and bulky side groups require a higher temperature to permit the same degree of mobility. Consequently, rigid thermoplastics with bulky side groups and strong secondary (intermolecular) bonds have high transition temperatures. Likewise, the very strong (intermolecular) covalent bonds of thermosets cause them to have higher rig s than many thermoplastics. For amorphous thermoplastics the maximum continuous use temperature consequently is slightly below Tg, whereas for thermoplastics with appreciable degree of crystallinity temperatures in excess of Tg and even close to Tm may be permissible for limited periods of time. Table 2.2 illustrates indicative transitions temperatures for some unreinforced, or neat, polymers as well as common or recommended processing temperatures, Tproc. In the unstressed state the molecules of a high-molecular-weight polymer liquid are heavily intertwined. For the liquid to flow requires that molecules move in relation to one another and the resistance to flow in a high-molecular-weight polymer liquid therefore is significant. However, if the liquid is sheared, the molecules are gradually aligned, fewer entanglements remain, and the resistance to flow (i.e. the viscosity) is reduced. On the other hand, if the molecular weight is moderate, i.e. the molecules are not excessively long, the resistance to flow is lower since there are not as many entanglements. In this case shear is unlikely to significantly lessen the degree of entanglement and thus will not affect the viscosity much. Besides temperature, the molecular weight of a polymer is therefore the single most important factor in determining its viscosity. The viscosity and the so-called shear-thinning, or pseudoplastic, tendency (i.e. that the viscosity is reduced by higher shear rates) increase rapidly with molecular weight. Since a higher temperature manifests itself in increased molecular mobility it strongly facilitates flow. A thermoplastic melt, which consists of high-molecular-weight molecules, is usually shear-thinning (see fig. 2.12, which shows the viscosity of PEEK). As further illustrated by the figure there is also a significant temperature-dependency. Table 2.2 gives typical zero-shearrate shear viscosities, r/0, for a few polymers only, since viscosity data usually are quite difficult to come by in the literature. However, the behaviors exhibited in fig. TABLE 2.2 Transition temperatures, processing temperatures, and viscosities of selected neat polymers [6-13]. The shear viscosities quoted are the zero-shear-rate values at the given temperatures
PP PA 6 PA 12 PA 6,6 PET PPS PEEK PEI PES PAI
Tg (~
Tm (~
Tproc (~
rio (Pa s)
-20--5 50-70 45 55-80 80 85 145 215 225 245-275
165-175 225 180 265 245-265 285 345
> 185 225-290 180-270 270-325 260-310 300-355 360-400 350-425 340-380 < 400
101-102 (230~
380 (38ooc) 103 (360~ > 105 (340~
Thermoplastic composite sheetforming
51
A 700 o
600 o.
500 7
.,~
400
o~
300
~
200 e.-
r
100 0 10 0
~ 101
~ 10 2
~.....~ 10 3
Shear Rate [l/s]
Fig. 2.12. Shear viscosity of molten PEEK as function of shear rate and temperature. Note the logarithmic shear-rate scale. Data from reference [10].
2.12 can be assumed indicative for thermoplastics while the magnitudes and degrees of temperature and shear-rate dependencies naturally vary from one polymer to another. In terms of most composites manufacturing operations a low viscosity is desirable, meaning that it may be tempting to increase the processing temperature based on the temperature dependency displayed in fig. 2.12. Although this temperature-dependency indeed is exploited for this purpose, it cannot be done indiscriminately. As previously mentioned, solid polymers eventually degrade through chain scission and crosslinking. This is even more so for molten thermoplastics since the molecular mobility is so much greater than in solid form, as well as the fact that the higher temperature stimulates chemical reactions. Figure 2.13 illustrates the allowable exposure time before onset of degradation for molten PEEK as function of temperature. The tolerance to degradation of PEEK is greater in the absence of oxygen, which is a
120 ~ ' 100 .n E ,80 0
"u E
60-
GI9 40 o 9 20
.E_ I-
0 360
In Air I
380
.....
I
400
,,,
I
420
~-- Temperature [~
Fig. 2.13. Time to surface degradation for PEEK as function of temperature in presence and absence of oxygen. Data from reference [14].
B.T. flstr6m
52
trait shared with most thermoplastics which readily oxidize if given the opportunity. The general trends exhibited in fig. 2.13 can be assumed indicative for thermoplastics. Heat transfer in polymers is due to thermal agitation across intramolecular and intermolecular bonds; the stronger the bond, the higher the conductivity. The coefficient of thermal conductivity (CTC) therefore increases with molecular weight, molecular alignment, and crystallinity. The CTC may increase or decrease with temperature depending on polymer. The specific heat, or heat capacity, arises from the freedom of movement of the molecules and thus decreases with crystallinity and increases with temperature, i.e. molecular mobility, and accordingly increases rapidly as Tg is passed. It was previously mentioned that since the crystalline morphology represents close-packing of the molecules the density of the crystal is higher than in the amorphous phase (see fig. 2.14). The figure further shows that the density dependency on temperature changes considerably as Tg is passed. This behavior may also be assessed in terms of CTE. The CTE of polymers tends to be a linearly increasing function of temperature both below and above Tg, but with a stronger temperaturedependency above Tg. Closely related to the CTE is the total volumetric shrinkage from melt (processing temperature) to solid (service temperature), which if not taken into account may lead to poor dimensional stability and sink marks. Table 2.3 gives thermal conductivity, k, specific heat, Cp, and CTE, c~, of some neat polymers. The table illustrates that the thermal properties do not vary drastically between polymers; this is essentially true also for thermosets. Since the data of table 2.3 apply at room temperature it is important to recall from the discussion above what happens as the temperature increases.
2.3.1.2. Mechanical properties Since crystals are stiffer than amorphous regions, stiffness increases with degree of crystallinity (see fig. 2.11). However, higher stiffness may also be obtained using
E3
I _
i
Liquid
r~
Fig. 2.14. Polymer density as function of temperature.
Temperature
Thermoplastic composite sheet forming
53
TABLE 2.3 Thermal properties of selected neat polymers [6,15,16]
PP PA 6 PA 12 PA 6,6 PPS PEEK PEI PES
k
G
(W/m ~
(kJ/kg ~
10-6 ~ -~
0.11-0.17 0.24 0.21-0.31 0.24 0.29 0.25 0.07 0.26
1.8-2.4 1.67 1.26 1.67 1.09 1.34
80-100 80-83 61-100 80 49 40-47 47-56 55
1.0
polymers featuring increased molecular rigidity, bulky side groups, and to a lesser degree increased molecular weight, although it should be remembered that such configurational traits impede crystal growth. Thus, if both high stiffness and high temperature-tolerance is desirable there will be a tradeoff between high transition temperatures and the degree of crystallinity, i.e. stiffness. Significantly, the thermoplastics with the highest mechanical properties and temperature-tolerance owe these traits to stiff molecular structures, which also deprive them of the ability to form crystals to any significant degree, i.e. they are amorphous. Thermosets typically are stiffer than thermoplastics due to the three-dimensional molecular structure bound together by covalent bonds. The strength of a material may be measured in so many different ways that sweeping statements about strength are difficult to make. However, the strength of polymers is highly dependent on and increases with the strength of intramolecular and intermolecular bonds, with the degree of crystallinity and, to a lesser degree, with molecular weight. Consequently, courtesy of the three-dimensional molecular structure, thermosets tend to have higher strength than thermoplastics. In general the relatively weak intermolecular forces of thermoplastics translate into a ductile material with high strain to failure, toughness, and damage-tolerance, since the molecules to a certain degree can slip relative to each other without rupturing covalent bonds. Since crystalline regions act as physical crosslinks, ductility decreases with increasing degree of crystallinity. Correspondingly, thermosets tend to be brittle and have low strain to failure, toughness, and damage-tolerance since the covalent bonds cannot yield much. Table 2.4 gives indicative mechanical properties of neat polymers. The table significantly illustrates that the differences in mechanical properties between polymers with the exception of the failure strain are not as significant as one might expect. Several properties other than thermal and mechanical may be of importance, depending on the intended application, e.g. electrical properties, optical properties, and tolerance to environmental exposure, but these are considered beyond the scope of this chapter.
54
B.T. ~lstrO'm
TABLE 2.4 Mechanical properties of selected neat polymers [16]. p denotes density, E elastic (Young's) modulus, a strength, and e strain to failure
PP PA PPS PEEK PEI PES PAI
p (kg/m3)
E GPa
cr (MPa)
e (%)
900 1,100 1,360 1,260-1,320 1,270 1,370 1,400
1.1-1.6 2.0 3.3 3.2 3.0 3.2 3.7-4.8
31-42 70-84 84 93 105 84 93-147
100-600 150-300 4.0 50 60 40-80 12-17
2.3.2. R e i n f o r c e m e n t s
While the composite matrix is normally responsible for properties such as temperature and environmental tolerance, the reinforcement primarily determines the composite's mechanical properties. The reinforcement typically has strength and modulus one to two orders of magnitude greater than polymer matrices. 2.3.2.1.
Thermal properties
Table 2.5 gives representative thermal properties of some reinforcement types. The table illustrates a couple of interesting differences in reinforcement properties. First, glass fibers are isotropic for reasons previously discussed. However, perhaps the most relevant property in this context is the negative longitudinal C T E of aramid and carbon fibers; while another is the high longitudinal CTCs of carbon, which for some carbon types even exceed the CTCs of the best metal conductors. The table further gives approximate m a x i m u m use temperatures Tmax. 2.3.2.2. M e c h a n i c a l p r o p e r t i e s
Table 2.6 gives representative mechanical properties of c o m m o n reinforcements, illustrating the vast range of reinforcement properties available. While table 2.4 illustrates that there are no excessively large variations in mechanical properties of TABLE 2.5 Thermal properties of selected reinforcements [16-20]. Indices l and t denote properties in longitudinal and transverse fiber directions, respectively kl
kt
(W/m ~ E glass S-2 glass Kevlar 49 (aramid) Carbon (PAN) Carbon (pitch)
Cp
(kJ/kg ~
0.87
0.87
0.041 7-70 100-520
0.048
0.825 0.737 1.42 0.7-0.9 0.7-0.9
otI
Tmax (~
ott
(10-6 ~ -~) 5.0 2.9 -2.3 -0.5--0.7 -0.9--1.6
5.0 2.9 41 7-10 7.8
350 300 250 600 500
Thermoplastic composite sheet forming
55
TABLE 2.6 Longitudinal tensile properties of selected reinforcement types [16,18,21,22]. The abbreviations for carbon
fiber types stand for high strength/strain, intermediate modulus, high modulus, and ultra-high modulus, respectively
E glass S-2 glass Kevlar 49 (aramid) Kevlar 149 (aramid) Carbon (HS/S) Carbon (IM) Carbon (HM) Carbon (UHM)
P (kg/m 3)
El (GPa)
~l (GPa)
6l (%)
2,520-2,620 2,490 1,440 1,470 1,700-1,900 1,700-1,830 1,750-2,000 1,870-2,000
73 86 131 186 160-250 276-317 338-436 440-827
3.4 4.5 3.6-4.1 3.4 1.4-4.93 2.34-7.07 1.9-5.52 1.86-3.45
4.88 5.7 2.8 2.0 0.8-1.9 0.8-2.2 0.5-1.4 0.4-0.5
matrices (with the exception of failure strain), there are certainly most significant differences in the mechanical properties of different reinforcement types. It is also noteworthy that the stiffer the fiber, the lower the strain to failure; it is thus not possible to have both high strain to failure and high modulus. The qualitative categorization of the multitude of carbon fibers in table 2.6 is obviously somewhat arbitrary and certainly partially contradictory, but it is nevertheless quite common in the composites industry.
2.3.3. Composites All properties discussed above pertain to the constituents on their own. When the constituents are combined into a composite they all lend some degree of their own properties to the composite; this is after all the underlying concept of a composite. Even if one does not take the overall part geometry into account, there are numerous variables in composites design, such as constituent types, fiber contents, fiber orientations, etc. It has therefore proved to be quite convenient to be able to approximately predict composite properties. The following sections will briefly look at basic relationships to predict some thermal and mechanical properties of the simplest possible composite form: the lamina. A lamina consists of a flat (or curved) assembly of unidirectional fibers or a fabric impregnated with a matrix (see fig. 2.15). Although the properties of unidirectionally reinforced composites of any crosssection may be predicted using these relationships, they will likely prove inadequate when trying to predict properties of composites with more complex geometries, as well as laminated composites composed of laminae stacked at different angles. While laminate theory is considered beyond the scope of this chapter the interested reader should encounter little problem locating one of the many textbooks covering this topic.
2.3.3.1. Prediction of thermal properties To enable determination of lamina properties from those of the constituents, several assumptions may be made; among the more common assumptions are that
B.T. /lstrSm
56
Fig. 2.15. Composite lamina.
matrix and fibers are isotropic. While glass fibers really are isotropic, carbon and aramid fibers clearly are not and it may also be questionable whether the matrix really is isotropic. Through micromechanics-based considerations one may derive expressions to determine the thermal properties of laminae. The longitudinal CTEs may be expressed as [23]:
Vfolf Ef @ VmOlmEm =
(2.1)
v j E j + VmEm
where V is volume fraction and indicesfand m refer to fiber and matrix, respectively. The transverse CTEs may similarly be written [23]:
o~, = Vfotf (1 + vf) + Vmotm(1 + Vm) - (Vfvf + Vmvm)O#
(2.2)
where v is Poisson's ratio and c~t is given by eq. (2.1). Equivalent expressions for the CTCs are [24,25]:
kt = Vfkf + Vmkm kfkm
(2.3) (2.4)
= Okm + Vmk
while the heat capacity may be expressed as [25]:
Up=
Vf pffpf -k- VmPmCpm Vfpf + Vmpm
(2.5)
2.3.3.2. Prediction of mechanical properties Micromechanics-based predictions of lamina mechanical properties are significantly more common than the thermal relationships quoted above. Employing the same assumptions as in the previous section, one may estimate the modulus of elasticity (Young's modulus) in the longitudinal direction as: Et = VuET + VmEm
(2.6)
Thermoplastic composite sheetforming
57
Equation (2.6) is sometimes called the parallel model and constitutes an upper bound for the modulus of a composite. The modulus in the transverse direction may be estimated as: Et -
ETEm
(2.7)
V:Em + VmE: Equation (2.7) is sometimes referred to as the serial model and may be regarded as a lower bound for the modulus of a composite. The parallel model may also be used to estimate the major (in-plane) Poisson's ratio and the serial model correspondingly may be employed to estimate the (inplane) shear modulus, although Poisson's ratios and shear moduli of fibers rarely are known. Comparisons with experimental data have shown that the parallel model yields reasonably accurate results, whereas the serial model predicts moduli considerably deviating from experimental data. It is also possible to predict the lamina strengths based on micromechanics considerations although such expressions require extensive assumptions, including that all fibers are perfectly parallel, have exactly the same properties (i.e. fail simultaneously), and are perfectly bonded to an isotropic matrix. In longitudinal tension one may express the strength as: =
+ Zm m
(2.8)
If the fibers are much stiffer than the matrix (which holds true for all common fiber-reinforced polymers) and the fiber volume fraction is significant (which is the case for all structural composites) the latter term in eq. (2.8) may be omitted. Since this strength expression is based on such highly ideal assumptions it is to be regarded as an upper bound for the strength; indeed it predicts strengths significantly higher than experimentally determined ones. A variety of equivalent expressions for transverse, shear, and flexural strengths have been derived and may be found in the pertinent literature, including textbooks on mechanics of composite materials (e.g. references [26] or [27]). Such textbooks also discuss the assumptions and accompanying weaknesses of the micromechanics models above, including other and more refined models, and invariably also describe how to determine the effective properties of laminates. Prediction of laminae and laminate properties using the equations above as well as other and more refined models no doubt is convenient in the early design stages. It cannot be overemphasized, however, that such predicted properties rarely are sufficient to finalize a design and experimentally determined properties are usually a necessity.
2.3.3.3. Experimentally determined thermal properties Since predictions rarely can replace experimentally determined properties entirely, this section and the next therefore attempt to give some examples of experimentally determined properties. Figure 2.16 shows the temperature-dependency of the thermal properties of unidirectionally reinforced carbon/PEEK, which probably is the most well-characterized thermoplastic-based composite to be found in the open
B.T. AstrSm
58
0.8-
8
0.7 o o
E
i
0.6
!
i
0.5
i
i
i
/ i ~ "
!
i
J
~ _ ! . . _ ! i
i
i
~
i
i
0.3
.
1620
.
{
6
I
5
i
._.J . . . . .
i i
i i
I
-
,
1.8
1600
.............................[..................................~
1580
.................................. ,,.................................... 9 i................................ ~................................. i ................ i i i I ' i i t *
1.4
156o
0 a~ ". "~
..................................i....................................~...................................T...........
1.2
t~.
.................................. i ...................................
0.8
i
!
i
.................................t ....................[.................................. ].......
i
j
i
1.6
'
-~-,
!
i
i
~0o 80
o
1.0
1520
o
&
r
1540
"7, o
0 o E
i ................................... i .............. J,....................
;
.... i !
i
I
................................. ] ..................................................
0.4
.~
!~
~Z-~-*-.I I
i
;
i ................. j ..... ;
........................ ~......................................... ~ ......................... ~ ............ t ............... 4 ................................. } i ! t ~ }
60
0
40 20
0 -200
--
J
i i i , t i , ..................................i..................................i ...................................i ..............,..................~...............................i..............., ................... i i i ~ i ! J ! i i i i ......................... ~.................................i ................................ l ................i ................................i............J..................
i
- 1 O0
'
0
i
i
,
i~
j
f
1.0 0.8 0.6
(9 o
0.4
.-.
0
...............J.............................~.............t ................... 0 . 2
100
Temperature
200
Tg
300
T,,, 400
0
[~
Fig. 2.16. Thermal properties of unidirectionally reinforced carbon/PEEK as functions of temperature at Vf = 0.61. Values for CTE in excess of 150~ are estimated. Tg and Tm indicated in graphs. Data from reference [21.
literature. Thermal properties of other material systems are difficult to find in the literature and one therefore often has to resort to using eqs. (2.1) through (2.5).
2.3.3.4. Experimentally determined mechanical properties In analogy with the previous section, this section also attempts to provide some representative property data for thermoplastic composites. Table 2.7 gives properties of composites manufactured from E glass/PP, E glass/PA 12, and carbon/PEEK prepreg. The glass/PP and carbon/PEEK composites were molded from unidirec-
59
Thermoplastic composite sheet form&g
TABLE 2.7 Mechanical properties of composites molded from E glass-reinforced PP, E glass-reinforced PA 12, and high-strength carbon-reinforced PEEK prepregs [2,28,29]. r is shear strength, G shear modulus, and I L S S interlaminar shear strength, while index l denotes longitudinal, t transverse and tensile, c compressive,f flexural, and 2. out of plane Matrix: Reinforcement type:
PP E glass
PA 12 E glass
PA 12 E glass
Reinforcement form:
UD
UD weave
Balancedweave
0.35 1,480 620
0.55 1,900 710 90
0.52 1,850 350 350
570
800 160
500 500
D
p
flit ott
rrtc rrtc
rrtf rrtf rt• rlt
"t't_l_ Ett Ell
Etf Etf Glt Gt! Gt_I_ ~31t Vl_l_ Vtl
(kg/m3) (MPa) (MPa) (MPa) (MPa) (MPa) (MPa) (MPa) (MPa) (MPa) (GPa) (GPa) (GPa) (GPa) (GPa) (GPa) (GPa)
27.5 22
44 7.2 38 8
26 26 22 22
(%)
ett ILSS
(%)
(MPa)
0.61 2,130 80 1,100 220
120 175 80 137 9.4
5.1 5.1 3.2 0.33 0.32 0.04 0.40 0.40
21t_l_ V_l_t
e,
PEEK High-strength carbon UD
2.1
1.5 2.2 47
1.6 1.6 42
tionally reinforced m e l t - i m p r e g n a t e d prepregs, while the glass/PA 12 composites were m o l d e d f r o m p o w d e r - i m p r e g n a t e d fabric prepregs of two different types. The prepreg d e n o t e d U D weave was a c r o w f o o t weave with 90 percent of the fibers in the warp direction and 10 percent in the weft direction, whereas the prepreg d e n o t e d balanced weave was a satin weave (with equal a m o u n t s of fibers in the two orthogonal directions). Table 2.8 illustrates how the increased handleability of c o m m i n g l e d materials is also likely to lead to composite properties inferior to those achievable with melti m p r e g n a t e d prepregs. The d r a w b a c k of c o m m i n g l e d feedstock is that it m u s t be m e l t - i m p r e g n a t e d during processing, which is a non-trivial p r o c e d u r e with such a high-viscosity p o l y m e r as P E E K . Similar tendencies should be expected with powd e r - i m p r e g n a t e d reinforcement.
B.T. AstrO'm
60
TABLE 2.8 Properties of composites molded from melt-impregnated and commingled carbon/PEEK feedstock [2] Product form
O'lt (MPa)
Elt (GPa)
Olc (MPa)
Elc (GPa)
o'tt (MPa)
Ett (GPa)
Melt-impregnated Commingled
> 1,172 > 782
132 127
1,175 865
113 115
91 64
8.9 8.9
Table 2.9 provides properties for components compression molded from glass/PP GMT. For all product forms listed, with the exception of the last one which has half the reinforcement longitudinally oriented, the properties should be reasonably isotropic in the plane.
2.4. Manufacturing techniques The term sheet forming may generously be thought of as including both sheet formation, or rather consolidation of the raw material into a so-called blank, and forming of this blank, or sheet, into a curved component. To date virtually all types of sheet forming have employed prepregs and with this raw material form one may think of the route from prepreg to final component as consisting of three basic steps: prepreg lay-up, prepreg consolidation, and sheet forming. In some cases two or even all three of these steps may be combined into one operation, but it is more common that all three steps are separate. The remainder of this chapter introduces the most common routes to achieve these steps, but the order of the techniques described in no way implies any preference in terms of technical or economical feasibility. It deserves to be pointed out that most of the techniques discussed below are known by more than one name and the designations used herein are not necessarily the most common ones. TABLE 2.9 Properties of composites molded from glass/PP GMT [30]. For the last GMT type (Wf --- 0.43) half of the reinforcement is longitudinally oriented. W denotes weight fraction. GMT type
Wf
Fiber length (mm)
p
O'lt Elt (kg/m 3) (MPa) (GPa)
Elt (%)
O'lf Elf (MPa) (GPa)
Powder-impregnated
0.25 0.30 0.35 0.40
12 12 12 12
1,070 1,120 1,160 1,220
75 86 96 105
4.0 4.5 5.2 5.9
3.3 3.0 2.8 2.7
130 140 150 165
4.8 5.5 5.9 6.4
Melt-impregnated
0.20 0.30 0.40 0.43
continuous continuous continuous continuous
1,020 1,130 1,190 1,210
55 85 105 250
3.5 4.5 6.0 10.5
1.8 1.8 1.7 1.7
90 110 140 160
3.5 4.5 5.5 8.5
Thermoplastic composite sheetforming
61
2.4.1. Prepreg lay-up The most straightforward way of laying up the prepreg plies to form a composite no doubt is to cut the prepreg by hand and likewise to lay it up by hand, ply by ply. Due to the research and development status of most sheet forming operations, this fully manual procedure is indeed the most common, although semiautomated or fully automated machinery used in the aerospace industry when dealing with thermoset prepregs certainly could be used with thermoplastic prepregs as well. With such machinery wide prepreg sheets would be automatically cut to size and then robotically stacked in the desired fashion. However, for such procedures to make financial sense, relatively large productions volumes would be necessary. In contrast, with continuous and quasi-continuous consolidation processes the prepreg lay-up becomes an integral part of the consolidation process. In such continuous processes the prepreg plies are continuously uncoiled from rolls and gradually consolidated, as further discussed in the following sections.
2.4.2. Prepreg consolidation Once the prepreg plies have been laid up the stack may be consolidated in several different fashions. The basic requirement on any consolidation technique for thermoplastic prepregs is to apply sufficient pressure to maintain the molten reinforcementmatrix mass in the desired shape for the time required to allow itJto become dimensionally stable. With thermoplastic prepregs this time is of the order of tens of seconds to a couple of minutes, since the part only needs to be cooled for the matrix to solidify. It has been shown that full consolidation of two thermoplastic layers may be achieved in a fraction of a second provided the layers are at sufficiently high temperature and instantaneously are brought into intimate contact. With thermoplastic resins the strength between two layers brought into intimate contact at a temperature in excess of Tg is governed by diffusion of polymer molecules across the interface between the two layers. Given sufficient time this diffusion process will lead to an interfacial strength equal to that of the virgin resin. The time to reach the virgin strength is strongly dependent on temperature, since higher temperatures promote diffusion. This healing process is referred to as autohesion, i.e. self-adhesion between two layers of the same thermoplastic resin. While autohesion has been achieved in very short time frames in laboratory composites consolidation experiments, it is rare that similarly short time frames are achieved in real processing operations. In most manufacturing situations it is not the time required to achieve virgin material strength over an interface that limits the processing rate; the limits are usually set by the time required to heat and cool the material.
2.4.2.1. Vacuum-bag consolidation Following established procedures for thermoset composites manufacture, it is naturally possible to vacuum-bag consolidate a prepreg stack, possibly using an autoclave. Figure 2.17 illustrates how the prepregs have been laid up onto a mold and then covered by a vacuum bag. Vacuum is then drawn under the bag to compact
62
B.T. flstr6m
Fig. 2.17. Schematic of vacuum-bag consolidation.
the prepreg stack with (the external) atmospheric pressure. The vacuum is maintained throughout a complete heating and cooling cycle and results in a fully consolidated laminate. Heating is likely achieved through placing the entire vacuumbag assembly, including mold, in an oven and - - following complete melting of the prepreg matrix - - subsequent removal of the assembly from the oven and back into open air to cool off. If an autoclave is used, higher compaction pressures may be achieved through pressurization of the internal atmosphere of the autoclave; heating would likely be achieved through heating of the same internal atmosphere. Whether an autoclave is used or not, the mold naturally may incorporate provisions for independent heating and cooling to increase process efficiency. Although vacuumbag consolidation is certainly technically feasible, it likely does not make economical sense in anything but laboratory-scale experiments due to the large degree of timeconsuming manual labor and - - if an autoclave is used - - the expensive equipment involved. However, hand layup of thermoset-based prepregs onto a contoured mold followed by vacuum bagging and autoclave consolidation is an established technique to manufacture shell-like composites that also has proven feasible with thermoplastic prepregs. In this case prepreg lay-up and conformation to the mold are combined into one step that is followed by vacuum-bag consolidation (with or without autoclave) without further forming. 2.4.2.2. Matched-die consolidation
A much more common and economically more sensible consolidation technique is to employ one or more hydraulic presses and consolidate the prepreg stack between parallel platens, possibly using a picture-frame mold to prevent resin bleeding from the edges of the laminate. One incarnation of this consolidation technique employs an oven to heat the prepreg to a temperature in excess of the softening point of the matrix, whereupon the prepreg stack is quickly transferred to a press equipped with a mold having a temperature below the softening point of the matrix. The press then very rapidly closes to apply sufficient consolidation pressure during cooling (see fig. 2.18). This consolidation technique is best suited for fully melt-impregnated prepregs and cycle times of less than a minute may be achieved assuming that the matrix is completely melted. The reason for the short cycle times is that with fully meltimpregnated prepregs consolidation is only a matter of squeezing the prepreg plies together to eliminate inter-ply gaps and then to allow for autohesion to occur before the matrix resolidifies.
Thermoplastic composite sheetforming
63
Fig. 2.18. Schematic of matched-die consolidation. For material forms that are not already fully melt-impregnated, e.g. powderimpregnated and commingled prepregs as well as unimpregnated reinforcement layers interleaved with resin films (called film stacking), the processing requirements are quite different. With such materials matrix flow relative to the fibers must be permitted to achieve full fiber wetting and a completely consolidated laminate. Due to the very high matrix viscosities involved this required time frame is significantly longer than that needed for consolidation of melt-impregnated prepregs. To provide such extended time for flow, either two presses and two sets of molds - - one heated and one cooled or a mold which allows both heating and cooling are required. With two presses the prepreg stack is placed in the heated mold, which then is closed to apply slight pressure until the desired equilibrium temperature (in excess of the softening point of the matrix) is reached within the material. When the specified molding temperature has been reached, molding pressure is applied for a given length of time. The heated mold is then opened and the molten material is rapidly transferred to the cooled mold where it is consolidated under pressure. With one mold having both heating and cooling capabilities the prepreg stack is placed in the unheated mold in the press which is then closed. As in the previously described technique the material is gradually heated under slight pressure until the desired temperature is reached when full molding pressure is applied; the mold is then cooled to consolidate the material. (These two techniques may be combined employing one mold and two presses. In this case the material remains in the mold which is moved from the heated to the cooled press.) Neither of these two techniques appear to have much potential for mass production of flat laminates due to the expensive machinery (two presses) and long cycle times; the former technique may possibly achieve cycle times of the order of ten minutes, whereas the latter has cycle times of the order of an hour.
2.4.2.3. Double-belt-press consolidation A DBP offers the only realistic means of continuously consolidating prepregs into wide laminates (see fig. 2.19). The prepregs enter the press and are heated under pressure until the matrix is molten, whereupon the laminate is cooled under pressure so as to exit the DBP fully consolidated. In this case prepreg lay-up and consolidation are essentially performed simultaneously since the incoming prepregs are
64
B.T. flstr6m
Fig. 2.19. Schematic of double-belt-press consolidation.
uncoiled from rolls of material through the forward motion of the bands of the DBP. On-line consolidation is a term that is sometimes used to describe such simultaneous lay-up and consolidation. This consolidation method is the only technique that appears to be economically feasible for large-scale blank manufacture. Linear consolidation speeds are of the order of a few millimeters per second. Any prepreg form may be continuously consolidated into a laminate with a DBP, but processing rates are likely to be lower with not yet melt-impregnated material forms.
2.4.2.4. Tape laying A significantly less common but nevertheless technically feasible technique to online consolidate flat laminates is tape laying. In this case prepreg in tape form is unrolled from a spool and continuously laid up onto the mold (see fig. 2.20). Both the mating surfaces are locally heated and joined under pressure so as to achieve continuous consolidation, or welding. If both the previously laid ply and the incoming prepreg tape have completely melted surfaces when they are joined, no separate consolidation step may be needed and the laminate thus is ready for demolding as soon as lay-up is completed. However, one may instead aim only for partial consolidation to ensure that the prepregs stay in place in relation to one another and then achieve full consolidation in a separate processing step, such as through any of
Fig. 2.20. Schematic of tape laying.
Thermoplastic compositesheetforming
65
the aforementioned consolidation techniques or concurrently with one of the forming techniques described later in this chapter. If only partial consolidation is the aim, the lay-up can proceed much more rapidly with the same amount of heating, thus increasing the processing rate. Tape laying may also be used to produce curved components, thus enabling one-step layup--consolidation-forming. However, due to the localized and highly nonuniform heating history of such a component most attempts at such one-step manufacture have resulted in considerable residual stresses causing component warpage. It is therefore common to combine tape lay-up with subsequent consolidation whether the component in question is a blank or a final component. 2.4.2.5. Intermittent matched-die consolidation The final consolidation technique described herein is intermittent matched-die consolidation as illustrated in fig. 2.21. In this technique the incoming prepregs are heated in an oven so as to melt the matrix (the oven may possibly be replaced by a press with a heated mold to mimic the two-press consolidation procedure described above). The molten material is then indexed to enter a press with a cooled open-sided mold, where it is consolidated. The mold then opens, the material is indexed, and the consolidation repeated. Since this consolidation technique is quasi-continuous it may hold a promise of being economically feasible for large-scale blank manufacture. 2.4.3. Sheet forming Once a fully consolidated blank manufactured through any of the aforementioned lay-up and consolidation techniques is available, there is a range of possible means to form it into an arbitrarily shaped component. Virtually all prepregs contain continuous and oriented fibers, which from a manufacturing point of view are inextensible and embedded in a lubricating liquid resin. The issue of conforming and subsequently reconsolidating a previously consolidated blank (or possibly an unconsolidated prepreg stack) is a non-trivial exercise. Figure 2.22 illustrates possible deformation modes of the plies that make up the blank (or the unconsolidated stack) and the minimum requirements in terms of flow mechanisms to achieve this mode of deformation. Since the blank predominantly is made to conform to the mold and the inextensible fibers allow very little flow, the blank is normally almost the
Fig. 2.21. Schematic of intermittent matched-die consolidation.
66
B.T. AstrO'm
Fig. 2.22. Hierarchy of deformation modes for stacked reinforcement plies and corresponding required flow mechanisms. Redrawn from reference [2].
same size as the final component (often larger) and the thickness change between blank and final component is small. In shaping of doubly curved components there is a pronounced risk of wrinkling of the plies during conformation. The wrinkling tendency is significantly reduced if the plies to be formed have shape and size resulting in as little excess material around the edges (that needs to be trimmed off in a secondary operation following molding) as possible. Another important means of reducing the risk of wrinkling is to keep the plies under slight tension during molding. In most of the following technique descriptions such tensioning devices are neither explicitly mentioned nor shown in the figures, but would nevertheless likely improve results in all techniques when forming doubly curved components. Correctly optimized most of the sheet forming techniques discussed below ought to be able to both form the final component and consolidate a previously unconsolidated prepreg stack in the same step. In practice this has proven difficult to achieve in many (but not all) techniques and it appears as if most work on sheet forming utilizes preconsolidated blanks as raw material. Use of preconsolidated blanks is clearly economically disadvantageous, but generally simplifies and speeds up processing and results in improved consolidation in the formed component. For reasons of overall process economy, one-step forming and consolidation ought to be an area most worthy of research.
2.4.3.1. Matched-die molding Matched-die compression molding, also known as stamping due to its close similarity with sheet metal stamping, employs matching metal dies, or molds, mounted in
Thermoplastic composite sheetforming
67
a press (see fig. 2.23). The general processing steps are similar to those in matched-die consolidation described above. An oven is used to heat the blank to a temperature in excess of the softening point of the matrix, whereupon it is quickly transferred to a mold having a temperature below the softening point of the resin. The press then very rapidly closes to force the blank to conform to the mold and then maintains sufficient pressure during component cooling to ensure that the material is reconsolidated in its new shape. Due to its short cycle times and similarity with compression molding of both sheet metal and thermoset composites, matched-die compression molding is seeing quite some interest, particularly from the automotive industry. Significant drawbacks of this technique are very expensive molds and that forming is so rapid that it is likely that only moderately curved components are manufacturable when the feedstock contains continuous and aligned fibers.
2.4.3.2. Rubber-die molding Rubber-die molding is closely related to matched-die molding; fig. 2.24 illustrates the concept. Rubber-die molding reduces the risk of wrinkles in the part through more evenly applied pressure. Due to the poor heat transfer characteristics of rubber the matrix solidifies less rapidly upon die contact than with metal dies and more deeply drawn components are thus manufacturable. To facilitate molding of more complex geometries the rubber block may be contoured to more or less match the shape of the solid lower mold half. The technique employs significantly cheaper molds than matched-die molding.
Fig. 2.23. Schematic of matched-die molding.
Fig. 2.24. Schematic of rubber-die molding.
68
B.T. ~lstrO'm
2.4.3.3. Hydroforming Another quite similar molding technique is hydroforming. In this process a liquid is contained by a flexible membrane that is capable of conforming to the shape of the other mold half (see fig. 2.25). Following mold closure the liquid is pressurized to force the blank to conform to the other mold half. For the same reasons as with rubber-die molding the cooling is relatively slow, thus allowing for longer forming times and consequently more complex contouring. Also hydroforming reduces the risk of wrinkles in the part through the hydrostatically applied pressure, which may be significantly higher than in rubber-die molding. Hydroforming employs cheaper molds than both the aforementioned techniques.
2.4.3.4. Deep drawing In deep drawing the material to be formed is mounted in a frame that keeps the material under slight tension until forming is completed (see fig. 2.26). As the molten material leaves the preheater it is placed over a female "mold", essentially consisting of a hole the shape of the projected area of the final product. A male mold then rapidly punches the pliable material through the hole of the female mold. This crude forming technique likely produces components with poor external surface finish and allows limited control of material movement during forming. Nevertheless, it is a low-cost method with lower tooling costs than the aforementioned techniques and has proven its commercial feasibility in, for example, manufacturing of hinge covers for civilian aircraft cargo areas.
Fig. 2.25. Schematicof hydroforming.
Fig. 2.26. Schematicof deep drawing.
Thermoplastic composite sheetforming
69
2.4.3.5. Diaphragmforming The only technique that has been developed exclusively for thermoplastic composites manufacturing is diaphragm forming, which may be seen as a refined version of conventional autoclave consolidation. The process has been investigated by numerous different organizations and the results are encouraging. Since diaphragm forming has been investigated by many, the technical solutions vary significantly; two of the more common versions are described in the following. The blank to be formed is placed between two flexible diaphragms. The diaphragms, but not the blank which remains free-floating, are clamped around the entire perimeter using a clamping frame and the air is evacuated between the diaphragms. Thus far in the description most versions of diaphragm forming remain the same; the main differences are in heating and forming techniques. In one diaphragm forming version the diaphragm-blank sandwich is placed in an oven and heated to a temperature in excess of the softening point of the matrix. The diaphragm-blank sandwich is then rapidly placed onto a one-sided female mold and vacuum is drawn in the space between the lower diaphragm and the mold and pressure is applied above the upper diaphragm to force the blank to conform to the mold (see fig. 2.27). Either vacuum and pressure or just one of them may be used in forming. Since the mold is normally unheated the component solidifies as it gradually comes in contact with the mold. In another incarnation of diaphragm forming the diaphragm-blank sandwich is placed on top of the mold and then this entire assembly is placed in an autoclave, which often is purpose-built. The internal atmosphere of the autoclave is then heated to melt the matrix whereupon the combined forces of vacuum below the lower diaphragm and pressure above the upper diaphragm make the blank conform to the mold. When forming is completed the heated gas surrounding the mold and the diaphragms is replaced with cool (ambient) air to solidify the component. More rapid processing may be achieved if the mold incorporates heating and cooling options. The first diaphragm material was superplastic aluminum, but most later work has employed polymer films, particularly PI, and sheet rubber. Rubber diaphragms have an advantage in that they may be reused a few times, whereas aluminum and polymer films may not be reused since they become permanently deformed. It is important that the processing temperature is such that the diaphragms allow large plastic deformations, which for polymer diaphragms translates into temperatures between
Fig. 2.27. Schematic of diaphragm forming.
70
B.T. ~lstrO'm
Tg and Tm. PEEK-based prepregs are thus very well compatible with PI diaphragms, whereas at the processing temperatures common with PP they do not allow sufficient deformation. With rubber diaphragms this is not a concern since they are pliable at all realistic forming temperatures, but instead the processing temperature must be below the upper use temperature of the diaphragms. Since low pressures are involved, simple tooling may be used. Materials include sheet metal which allows rapid temperature changes and, for experimental work, plaster and wood molds, which have their predominant advantage in the low cost. The main characteristic of diaphragm formed components is that they may be deeply drawn and quite complex, especially when forming in an autoclave. This is partly due to the diaphragms keeping the material both under tension and under slight lateral compression and partly due to the matrix being pliable for a long time (basically until it comes into contact with the mold in the first technique and for any desired time in the latter technique). Due to its versatility the scope for commercial applications of diaphragm formed components should be great, but the commercial acceptance of the technique remains to be seen. Components that appear to be nearing commercial reality are glass/PP blister fairings and leading edges for jet engines to replace hand-laid-up and autoclave-consolidated carbon/epoxy components. 2.4.3.6. Folding Folding is a sheet forming technique different from the previously discussed ones in that it only involves localized heating and forming. Blanks may be folded through heating along a line and subsequent bending along this line (see fig. 2.28). Despite the fact that continuous fibers are likely to buckle or fracture, folding even of honeycomb sandwich panels, where the core ends up being crumpled has proven commercially viable in manufacturing of for example parts for aircraft interiors. 2.4.3.7. Roll forming Roll forming, which just like matched-die molding has been borrowed from sheet metal forming, is the only potentially continuous sheet forming technique. In roll forming several consecutive pairs of contoured rollers, normally four or more, gradually deform the molten blank to the desired shape (see fig. 2.29). The rollers, which are driven, are normally unheated and they consequently gradually cool the component. Roll forming is potentially capable of manufacturing any constant cross-section geometry and the products may be curved if desired. Nevertheless, so far thermoplastic roll forming has been used to manufacture hat and Z shapes only. Compared to most of the previously mentioned manufacturing techniques, little
Fig. 2.28. Schematicof folding.
Thermoplastic composite sheet forming
71
Fig. 2.29. Schematic of roll forming.
work on roll forming of thermoplastic composites appears to be ongoing despite the feasibility of the technique having been proven.
2.4.3.8. Matched-die molding of GMT In composites applications the term sheet forming is usually used to refer to conformation of a flat blank reinforced with aligned and continuous reinforcing fibers to a mold. In contrast, in matched-die molding using GMT as raw material the materialflows (rather than conforms) to fill the mold, since there are normally no aligned and continuous fibers to effectively prevent flow and also due to the fact that the fiber content is lower than in prepregs. While matched-die molding of GMT therefore may be slightly beyond the scope of this chapter, it is the only technique to manufacture shell-shaped structural thermoplastic composites that is currently in widespread commercial use and it has therefore been included for reference. The technique employs presses and molds similar to the previously described technique of matched-die molding. The main difference from fig. 2.23 is that in this case the heated raw material does not already cover most of the mold; instead the so-called charge covers only about half the mold area and the closing mold forces the charge to flow to fill the mold (see fig. 2.30). Since the GMT flows to fill the mold a component molded from GMT may have varying thickness and, for example, bosses and ribs, which are features difficult to obtain with matched-die molding of continuous-fiber-reinforced blanks. Since the material flow is notable the reinforcement is oriented in the direction of the flow and properties therefore may vary significantly within a component. In applications where increased stiffness is required GMT with varying degrees of oriented and possibly continuous reinforcement or interleaved unidirectionally reinforced prepregs may be used, thus partially bridging
Fig. 2.30. Schematic of matched-die molding of GMT.
72
B.T. ~lstrO'm
the gap between matched-die molding of GMT and matched-die molding of continuous-fiber-reinforced blanks. The biggest users of GMT are automobile manufacturers, particularly European ones. GMT-based composites are notorious for their poor surface finish and are consequently often hidden from direct view in under-hood applications and in for example seat frames.
Acknowledgement The author gratefully acknowledges that the bulk of this chapter was written when he was a Visiting Senior Lecturer at the Department of Mechanical Engineering at the University of Auckland, New Zealand.
References [1] Thermoplastic Composites Materials Handbook, ICI Composites, Inc., USA, 1991. [2] Cogswell, F.N., Thermoplastic Aromatic Polymer Composites, Butterworth-Heinemann, Oxford, UK, 1992. [3] Jang, B.Z., Advanced Polymer Composites: Principles and Applications, ASM International, Materials Park, OH, USA, 1994. [4] Caldwell, D.L., Interfacial Analysis, in Handbook of Composite Reinforcements, Ed. S. M. Lee, VCH Publishers, New York, NY, USA, 1993. [5] Tobolsky, A.V., Properties and Structure of Polymers, John Wiley & Sons, New York, NY, USA, 1960. [6] Shalaby, S.W. & Moy, P., Thermal and Related Properties of Engineering Thermoplastics, in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 445-459, 1988. [7] Galanty, P.G., and Richardson, J.J., Polyethylene Terephthalates (PET), in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 172-176, 1988. [8] Brady, D.G., Polyphenylene Sulfides (PPS), in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 186-191, 1988. [9] Data Sheet 2: Making Consolidated Sheet from Aromatic Polymer Composite, APC-2, ICI Fiberite Corporation, 1987. [10] Taske II, L.E., Personal communication, BASF, Charlotte, NC, USA, 1990. [11] Fines, R.E. & Bartolomucci, J.P., Polyether-imides (PEI), in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 156-158, 1988. [12] Watterson, E.C., Polyether Sulfones (PES, PESV), in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 159-162, 1988. [13] Fitzpatrick, J.E., Polyamide-imides (PAl), in Engineered Materials Handbook, Volume 2, Engineering Plastics, ASM International, Metals Park, OH, USA, 128-137, 1988. [14] The Thermal and Oxidative Thermal Degradation of APC-2, ICI Composites, Inc. [15] Modern Plastics Encyclopedia '95, McGraw-Hill, New York, NY, USA, 1995. [16] Hancox, N.L. & Mayer, R.M., Design Data for Reinforced Plastics- A Guideline for Engineers and Designers, Chapman & Hall, London, UK, 1994. [17] Anon., Fibers, in Engineered Materials Handbook, Volume 1, Composites, ASM International, Metals Park, OH, USA, 360-362, 1987. [18] Bunsell, A.R., Fiber Reinforcement, in Handbook of Composite Reinforcements, Ed. S. M. Lee, VCH Publishers, New York, NY, USA, 199-217, 1993. [19] Morgan, R.J. & Allred, R.E., Aramid Fiber Composites, in Handbook of Composite Reinforcements, Ed. S. M. Lee, VCH Publishers, New York, NY, USA, 5-24, 1993.
Thermoplastic composite sheetforming
73
[20] Diefendorf, R.J., Carbon/Graphite Fibers, in Engineered Materials Handbook, Volume 1, Composites, ASM International, Metals Park, OH, USA, 1987. [21] Pigliacampi, J.J., Organic Fibers, in Engineered Materials Handbook, Volume 1, Composites, ASM International, Metals Park, OH, USA, 54-57, 1987. [22] Miller, D.M., Glass Fibers, in Engineered Materials Handbook, Volume 1, Composites, ASM International, Metals Park, OH, USA, 45-48, 1987. [23] Shapery, R.A., Thermal Expansion Coefficients of Composite Materials Based on Energy Principles, Journal of Composite Materials, 2 (1968) pp. 380-404. [24] Rosen, B.W., Thermomechanical Properties of Fibrous Composites, Proceeding of the Royal Society of London, A319 (1970) pp. 79-94. [25] Taylor, R., Thermophysical Properties, in International Encyclopedia of Composites, Ed. S. M. Lee, VCH Publishers, New York, NY, USA, 5, 1-7, 1991. [26] Eckold, G., Design and Manufacture of Composite Structures, Woodhead Publishing, Cambridge, UK, 1994. [27] Daniel, I.M. & Ishai, O., Engineering Mechanics of Composite Materials, Oxford University Press, New York, NY, USA, 1994. [28] Plytron GN 638 T, Unidirectional Glass-Fibre/Polypropylene Composite, Borealis, Stathelle, Norway, 1995. [29] Product Information Vestopreg, HOls AG, Marl, Germany, 1994. [30] Berglund, L.A. & Ericson, M.L., Glass Mat Reinforced Polypropylene, in Polypropylene: Structure, Blends and Composites, Volume 3, Composites, Ed. J. Karger-Kocsis, Chapman & Hall, London, UK, 202-227, 1995.
This . Page Intentionally Left Blank
Composite Sheet Forming edited by D. Bhattacharyya 9 Elsevier Science B.V. All rights reserved.
Chapter 3
Computer Simulation of Thermoforming B.L. K O Z I E Y and M.O. G H A F U R Polydynamics Inc., 1685 Main St. West, Suite 305, Hamilton, Ontario, Canada L8S 1G5
J. V L A C H O P O U L O S and F.A. M I R Z A Faculty of Engineering, McMaster University, Hamilton, Ontario, Canada L8S 4L7
Contents Abstract 75 3.1. Introduction 76 3.2. Sheet production 77 3.3. Thermoforming simulation 78 3.3.1. Finite element formulations 80 3.3.1.1. Membrane formulations 80 3.3.1.2. Thick sheet formulations 82 3.3.2. Material behaviour 83 3.3.2.1. Non-linear elastic models 83 3.3.2.2. Visco-elasticmodels 85 3.3.3. Thermoforming simulation examples 86 3.4. Concluding remarks 88 References 88 Abstract This chapter provides a description of the application of the finite element method to the simulation of the thermoforming process. The objective of thermoforming simulation is the provision of a rational means of mold design and to also allow for the design of "optimal" final parts using the minimum amount of material. This can be achieved by comparing the simulated behavior using various materials and mold configurations with varying process conditions. This eliminates the need to perform inefficient and expensive "trial-and-error" procedures. A "state-of-the-art" review of the finite element method in the simulation of thermoforming is given. The review covers the details of the membrane and thick sheet finite element formulations as well as non-linear elastic (Ogden, Mooney-Rivlin) and visco-elastic (K-BKZ) material constitutive relationships. Some examples, giving comparisons between simulation results and experimental values are also included. Good agreement was obtained between the predicted and measured thickness distributions. The results 75
B.L. Koziey et al.
76
also indicate that the choice of material model (non-linear elastic versus visco-elastic) must be done carefully if reliable predictions of the thickness distribution are to be achieved. For straight thermoforming into shallow molds a non-linear elastic model is suitable. However, when deep drawn forming, complex mold geometry or plugassistance is involved, a visco-elastic model is required to obtain accurate predictions. 3.1. Introduction
The term "thermoforming" describes a number of related polymer processing techniques, in which thermoplastic sheets are softened by heat and subsequently formed by the application of vacuum, pressure, or a moving plug. The sheet may be stretched over a male mold (positive forming) or into a female mold (negative forming). On contact with the mold heat is lost and the material regains stiffness as it cools. The vacuum and plug-assisted forming processes are depicted in figs. 3.1 and 3.2, respectively. For a detailed description of thermoforming operations, equipment design as well as heating and cooling issues refer to Throne [1]. Geometries of thermoformed products are usually simple (boxes, food trays, various containers, refrigerator liners, but lately also computer casings). Thermoforming competes with blow molding and injection molding. The main advantages of this process are (i) the relatively low cost of thermoforming machines and the very low cost for the molds, and (ii) it is easy to form large area thin section parts. The disadvantages are (i) limited product shapes, (ii) difficulties in obtaining the required thickness distribution, (iii) it is difficult to control molecular orientation, and (iv) limitations in service temperature which may induce strain recovery or shrinkage. In thermoforming the final part thickness is typically controlled by employing differential heating of the plastic sheet and plug assistance. The critical parameters associated with these techniques for controlling the final part thickness have generally been determined by trial and error. Unfortunately this has meant that the A
plastic sheet
B
!
.... Clamp
.
Vacuum holes
// . .l
.
.
.
.
.
.
V
Vacuum
Fig. 3.1. Vacuum forming: (A) preheated clamped sheet over female mold prior to forming; (B) vacuum applied.
Computer simulation of thermoforming A
..................
Clamp
N~
Air
B
77 Air
C
"/" "
Plastic Sheet
T Vent
I Vent
Fig. 3.2. Plug-assist thermoforming: (A) preheated clamped sheet; (B) sheet stretched with plug advance; (C) pressure applied to complete forming.
development of new mold designs and evaluation of thermal process parameters has been inefficient and expensive. Furthermore, a "trial-and-error" process does not allow a quick comparison to be made between competing mold designs and different materials. The objective of computer simulation of thermoforming is the provision of a rational means of mold design and to also allow for the design of "optimal" final parts using the minimum amount of material. This can be achieved by comparing the simulated behavior using various materials and mold configurations with varying process conditions. In this chapter a review of the use of the finite element method in the simulation of the thermoforming process is presented. Because thermoplastic sheet is essential to the thermoforming process a brief description of the primary sheet production methods is given. This is followed by a description of the problems facing the thermoforming industry and what can be hoped to be gained through mathematical modeling of the thermoforming process. A "state-of-the-art" review of the finite element method in the simulation of thermoforming is then given. The review covers the details of the various finite element formulations and material constitutive relationships used. Some examples, giving comparisons between simulation results and experimental values are also included.
3.2. Sheet production Thermoplastic sheet is essential to the thermoforming process. Thermoforming sheet is loosely categorized as thin-gauge (sheet thickness less than 0.25 mm) and thick-gauge (medium-weight sheet: 0.25-1.5 mm; heavy-gauge sheet: greater than 1.5 mm). Thin-gauge sheet is usually produced by the process of calendering while thickgauge sheet is usually produced by the process of extrusion [2] using a coathangershaped die or by calendering [2]. Thermoplastic sheets are manufactured in a variety of widths and lengths and usually come in a variety of predetermined thicknesses. In
78
B.L. Koziey et al.
general all thermoplastic resins that can be processed into a sheet can be thermoformed. Most of the fully developed thermoforming markets have been with amorphous [3] resins such as PVC, HIPS, PS, ABS, HDPE, PET, PETG, PP, PVDC, EVOH, PMMA. Amorphous plastics are suitable for thermoforming above the glass transition temperature Tg (usually 30~ to 60~ above Tg). These materials can be processed quite successfully over a wide temperature range. For semi-crystalline and reinforced amorphous materials such as PET and HIPS the forming window is very narrow and in general a higher forming pressure is required. For semi-crystalline materials the temperature should be just above the melting point Tm. The most common and versatile sheet manufacturing technique for thermoforming sheet production is extrusion. In extrusion, polymer pellets are drawn from a hopper into the gap between a heated barrel and a rotating screw. The mass of compacted solid pellets is transported forward and melted under the action of friction and heat. The polymer melt is then pumped through a die, usually of coathanger geometry, to produce a flat sheet which is then cooled and sized to proper gauge. The geometry is designed to allow the melt to flow downstream and laterally simultaneously so that a sheet of uniform thickness is produced. The sheet may be pulled mechanically by a roll stack as it exits the die. This not only reduces the gauge of the sheet, it also produces molecular orientation of the sheet in the machine direction. In most cases this imbalance in the orientation causes problems in the thermoforming process. This is especially true when the parts that are thermoformed are extremely deep or complicated. When the orientation is balanced biaxially on a specially configured extrusion line the strength and impact resistance of the sheet can be significantly increased. The other major process is calendering in which the molten polymer is converted into a sheet by a pair of rotating rolls. The melt forms a characteristic melt bank and spreads as it is squeezed between the rolls. Common calender roll arrangements include the L or Z configurations. A fixed gap is set between the initial rollers which is then continuously reduced between subsequent rollers until the desired gauge is achieved. Unlike sheets produced by the extrusion process those produced by the calendering method have no significant molecular orientation. A considerable amount of information is available in the literature on modeling and simulation of plasticating screw extrusion, flow through flat dies and calendering. The reader is referred elsewhere for more details [4-7].
3.3. Thermoforming simulation The current problems facing the thermoforming industry lie mainly with large wall thickness variations throughout the part with corners typically ending up as the thinner regions. Other problems include physical instabilities during inflation mainly rupture of the sheet as well as shrinkage and warpage of the final part. All these problems have an enormous effect on the performance and cost of a part. Non-uniform wall thickness variations and sheet rupture can be thought of arising for two main reasons, namely, mold geometry and process conditions. Other factors
Computer simulation of thermoforming
79
affecting the wall thickness include the initial dimensions of the sheet, temperature distribution on the surface of the sheet, stretch-strain material properties of the resin, inflation dynamics, and the cooling and solidification phenomena that occur in the mold cavity. Mathematical modeling can provide valuable insights into mold design and process improvement by aiding in the selection of new mold designs, by simulating the behavior of plausible mold configurations, and providing rational means for comparing the formability of different polymeric materials in a given thermoforming process. Such capabilities eliminate the need to perform expensive trial-and-error procedures, in order to optimize the resin distribution and minimize the peripheral waste. Advances in computer technology and numerical methods have made it possible to simulate complex forming problems. The advantages of using the finite element method over any other numerical method are twofold: first, the formulation is not restricted to any particular geometry and, second, the highly non-linear behavior can be directly accommodated into the method. Many difficult aspects of finite element modeling must be addressed in the analysis. These include, but are not limited to, large strains, large deformations, non-linear material behavior, incompressibility, contact between polymer and mold wall, physical and numerical instabilities during inflation, and time-dependent material and thermal effects. While some of these issues, such as large strains and large deformations, must be dealt with rigorously in the formulation, others such as contact between the polymer and mold wall can be included in a simplified manner without adversely affecting the accuracy of the model. The determination of what aspects of the thermoforming process should be included, excluded, or simplified in the finite element formulation is largely dependent on the specifics of the problem to be analysed. For example, for shallow pressure or vacuum forming, in which the forming of the sheet often occurs very quickly, the viscous behavior of the material may not be significant. However, in plug-assisted and deep drawn thermoforming, the forming operation usually takes longer, so the inclusion of time-dependent material effects (visco-elastic) may have a significant influence on the final results. Because of the limited amount of data available these decisions have to be based on engineering judgment and practical experience. A survey of the early work on the application of the finite element method to the simulation of the thermoforming process is given by Zamani et al. [8]. Their review covers the period between 1966 and 1988. In general, these early applications were found to be successful for the problems to which they were applied. However, the usefulness of the models developed as design tools, and their applicability to general thermoforming problems was not well established because of the limited range of problems investigated. These works, however, were very important since they established the basis for much of the future research efforts. Since that time the finite element models have increased in complexity, and more rigorous and comprehensive comparisons between simulation results and actual measurements have been made. As a result the currently available finite element models have become useful design tools allowing for optimization of resin distribution and minimization of peripheral waste. Furthermore, they also provide a means
80
B.L. Koziey et al.
of comparing the formability of various polymers under different temperature and pressure conditions. A "state-of-the-art" review of the finite element method in the simulation of thermoforming is given in the following sections. The review covers the details of the various finite element formulations and material constitutive relationships used. Some examples, giving comparisons between simulation results and experimental values are also included.
3.3.1. Finite element formulations In the finite element method the body to be analyzed is divided into a number of small subdivisions, or finite elements. The variables to be approximated are interpolated within each element using shape functions. Provided that the governing differential equations or a variational principle exists, finite element equations can be constructed from which an approximate solution for the process to be modelled can be obtained. Many texts are available on the finite element method and its application. For more information refer, for example, to Oden [9], Bathe [10], and Zienkiewicz and Taylor [11,12]. In the simulation of the thermoforming process there are two distinct types of finite element formulations: those which employ the membrane approximation, and those without the membrane assumption, i.e. thick sheet formulations. Each formulation has certain advantages and disadvantages. These will be described below, along with the details of each approach.
3.3.1.1. Membrane formulations In membrane formulations the bending resistance of the hot polymer is neglected and the sheet thickness is assumed to be very much smaller than its other dimensions. This assumption is quite reasonable for the bulk of the structure except possibly near clamping devices where the sheet may experience substantial bending. The majority of the finite element models formulated for the simulation of the thermoforming process employ the membrane approximation. See for example the work of Allard et al. [13], Warby and Whiteman [14], Nied et al. [15], deLorenzi and Nied [16], Taylor et al. [17], and Kouba et al. [18,19]. In general, the motion of the membrane is referred to a fixed Cartesian coordinate system. The position vectors of an arbitrary point P on the membrane surface in the current and reference configurations are denoted by ~ and ~', respectively. They are related through the expression ~ = X + 5, where 5 is the displacement vector. Since the resulting finite element equations will be non-linear they must be solved in an incremental manner. This is done by referring all variables to a previously calculated known equilibrium configuration and then linearizing the equations so that an approximate solution for the new configuration can be obtained. The solution can then be improved by iteration. Typically either the initial configuration at time 0, or the latest equilibrium configuration at time t are used as possible reference configurations. If all static and kinematic variables are referred to the initial configuration the formulation is referred to as a Total Lagrangian (TL) formulation. If all variables are referred to the last equilibrium configuration the formulation is referred to
Computer simulation of thermoforming
81
as an Updated Lagrangian (UL) formulation. The choice of which formulation to employ usually depends on the type of constitutive relation used. Since the constitutive relations typically used in thermoforming simulations are of the hyperelastic type, for example Mooney-Rivlin [20], Ogden [21], and the visco-elastic K-BKZ model the TL formulation is frequently employed. In this case the appropriate energy conjugate stress and strain measures are the second Piola-Kirchhoff stress tensor S, and the Green-Lagrange strain tensor E. The Green-Lagrange strain tensor is defined as 1
E-~(C-I)
(3.1)
where C is the right Cauchy-Green deformation tensor and I is the identity tensor. The constitutive relationship is usually expressed in terms of the principal stretches ~'i of the right stretch tensor U, or the invariants of the deformation tensor C. The invariants of the deformation tensor are easily calculated. To determine the principal stretches the eigenvalue problem for the Cauchy-Green deformation tensor, which is related to the right stretch tensor by U = C, must be solved. This yields two of the principal stretches, )~1 and ,~2, the third principal stretch ,k3 normal to the membrane surface, is determined using the incompressibility constraint )~1~,2~. 3 = 1. The incompressibility constraint in terms of the invariants of the deformation tensor is written as 13 = detC = 1. In membrane formulations the incompressibility condition is always satisfied. Typically the finite element equations are derived using the virtual work principle which requires that the rate of internal virtual work is equal to the external virtual work for an arbitrary velocity field satisfying the kinematic boundary conditions [9]. Assuming that the inertia and body force terms can be ignored the virtual work expression for the deformed membrane using a TL description is given by / S "6Eh0 d A 0 A0
dA
(3.2)
A
where A and A0 are the areas of the deformed and undeformed membranes, respectively. The applied pressure is denoted by p while t7 defines the vector normal to the surface of the deformed membrane, h0 is the initial membrane thickness and 6 is the membrane velocity vector. The finite element equations of equilibrium required for the incremental analysis are obtained through variation and linearization of the virtual work expression, eq. (3.2), followed by the introduction of the finite element discretizations. The elements used for discretization of the membrane typically [16,18] employ linear variations of the displacements within the element. In addition, the elements are usually triangular which allows curved edges to be more easily modeled. As mentioned previously the resulting finite element equations are solved using an incremental procedure. Starting from a known equilibrium configuration, usually the initial undeformed state, a small load increment is applied and the displacement increments are found. The solution is improved by applying an iterative method,
82
B.L. Koziey et al.
usually the standard Newton-Raphson method. Since the geometry of the membrane can often change drastically even for small load increments the load vector and stiffness matrix are recalculated during the iteration procedure using the updated geometry while keeping the load constant. After several iterations the incremental deformations become less than some prescribed value at which point the solution is considered to have converged. In the presence of a mold, collision calculations are continuously made to determine whether a node has contacted or penetrated the mold surface. When this occurs within a prescribed tolerance the node is permanently fixed to the mold surface at the contact point. This most closely approximates the actual forming conditions in which very little slip between the polymer and mold is observed. The load is incremented and the iterative procedure repeated until the desired pressure has been reached or all nodes have contacted the mold surface. The two most extensive membrane models of the thermoforming process are those developed by deLorenzi and Nied [16] and Kouba et al. [18,19]. Both employ similar finite element formulations; however, the model developed by Kouba et al. includes both non-linear elastic and visco-elastic material models, while that developed by deLorenzi and Nied includes only non-linear elastic material behaviour. In addition, the model of Kouba et al. includes pre-stretching of the sheet in a plug-assisted thermoforming process. This cannot be simulated using the deLorenzi and Nied formulation. A more detailed description of the various material models employed in thermoforming simulation is given in section 3.3.2. 3.3.1.2. Thick sheet formulations In a thick sheet formulation the bending resistance of the sheet is not assumed to be negligible as in a membrane formulation. Consequently, in addition to inplane shearing and extension of the sheet, transverse shearing and bending effects are also included in the model. This means that the strains and stresses will not be constant through the sheet thickness but will vary. While this provides a more accurate model of the sheet deformation the formulation of a thick sheet finite element model is much more complex than a membrane formulation. The added complexity is due to the fact that, (i) the incompressibility condition in a thick sheet formulation cannot usually be satisfied exactly but must be imposed through some type of numerical constraint (e.g. penalty method or Lagrange multipliers), and (ii) a thick sheet finite element model is inherently more complex than a membrane model. Perhaps the earliest thick sheet finite element model was that developed by Oden [9] which was used to simulate the free inflation of a sheet of finite thickness assuming non-linear elastic material behavior. The model was however not extended to include a mold so the thermoforming process could not be simulated. It was not until very recently with the work of Song [22,23] and Igl and Osswald [24] that thick sheet finite element models were applied to thermoforming process simulation. Igl and Osswald used a one-dimensional shell finite element model to study the thermoformability of wood-fiber-filled polyolefin composites. Song developed an axisymmetric thick sheet finite element model which can simulate straight and plug-assisted thermoforming assuming a non-linear elastic material response. While these
Computer simulation of thermoforming
83
simulations were found to be successful the added complexity of the thick sheet formulation is only important in some problems. In typical thermoforming problems the membrane approximation was found to predict results very close to those given by the thick sheet model even for relatively thick sheets [18]. The main advantage of the thick sheet models is that localized effects, such as bending and shearing near clamping devices and in corners, and stress concentrations near a plug boundary can be predicted. In typical thermoforming operations these effects will not dominate and thus the added complexity and computational effort required by thick sheet models is difficult to justify.
3.3.2. Material behaviour
For a material model to be applied successfully in a numerical simulation it must be capable of describing the material response under actual processing conditions. Ideally it should give a good representation of the stress-strain behavior of the plastic for both small and large strains, and over a wide range of temperatures and strain rates. During inflation into the mold cavity the sheet is mainly subjected to biaxial stretching. Consequently, the elongational characteristics of the polymer play an important role in the thermoforming process. From industrial experience the strain hardening characteristics of the plastic have been found to significantly affect the final thickness distribution of the finished product. Throne [1] states that the elastic modulus for materials in thermoforming is typically between 0.07 MPa and 1.0 MPa. Strain rates observed in the process normally range from 0.1 s-~ to 10 s-1. It is generally recognized that thermoplastics in a semi-molten state possess a strong viscous component which allows them to flow when sufficient stress is applied. They also possess a significant elastic component that resists flow and imparts integrity and self-supporting properties to the sheet. As a result in finite element simulations of thermoforming the polymer behavior is typically modeled using either a non-linear elastic or a visco-elastic constitutive model.
3.3.2.1. Non-linear elastic models
There is strong experimental evidence [25-27] that when polymers are extended at relatively high strain rates, at temperatures above the glass transition temperature their behavior can be adequately modeled using constitutive equations originally developed for rubber-like materials. It has also been shown experimentally [28] that the mechanical behavior of polymer materials above the glass transition temperature is essentially incompressible. The assumption of non-linear elastic material behavior greatly simplifies the formulation of the finite element equations, but neglects the viscous component of the polymer response. In non-linear elasticity the components of the constitutive tensor are given in terms of certain material constants, and are also functions of the material strains. For more information on non-linear elasticity refer, for example, to Green and Zerna [29], Green and Adkins [30], and Eringen [31].
B.L. Koziey et al.
84
For an isotropic material the stress-strain relationship is frequently defined using a strain energy function, W, given in terms of the Green-Lagrange strains. Such a material is referred to as a hyperelastic material and the stresses are given by OW S = ~ aE
(3.3)
where S is the second Piola-Kirchhoff stress tensor. Once an appropriate form of the function W has been defined the stresses can be evaluated. The determination of W must be done carefully to ensure that the frame indifference requirement is satisfied. Two different definitions of W which have been used almost exclusively in thermoforming simulations are the Mooney-Rivlin model and the Ogden model. Mooney-Rivlin model. In the Mooney-Rivlin [20] model it is assumed that the strain energy density function, W, for an incompressible material can be expressed as a polynomial function of the first two invariants, I1 and 12, of the Cauchy-Green deformation tensor, C. The generalized form of the strain energy function is given by [201 M
W - Z
N
Z
Aij(I1 - 3)i(I2 - 3) j
(3.4)
i=0 j=0 where A O. are experimentally determined constants. When the body is undeformed the strain energy W = 0 and constant A00 = 0. If only the first two terms, A10 and A01, are retained then the standard Mooney-Rivlin expression is obtained which is written as W -- A10(I1 - 3) + A01 (I2 - 3)
(3.5)
When A01 = 0 the model is referred to as the neo-Hookean model. The components of the stress tensor S can be calculated by substituting eq. (3.5) into eq. (3.3) and performing the required differentiation. Note that the stress normal to the membrane surface, $33, is assumed to be negligible. Ogden model. In the Ogden [21] model the strain energy density, W, is assumed to be a function of the principal stretches, instead of the invariants of the deformation tensor, and is given by m
W-
~/z__~n(,k~n + Z2" + Z3n _ 3)
(3.6)
n=l 0r
where Z l, ~'2 and )~3 are the principal stretches. Constants lZn and an are determined by fitting the model to experimental stress-strain data and can be either negative or non-integer values. However, the constants must yield a positive strain energy density function. Note that, because incompressibility is assumed, the third principal stretch, ~3 is expressed in terms of ~'1 and ~'2 using the constraint ~.1~.2~.3 = 1. The summation over n in eq. (3.6) extends over as many terms as are necessary to characterize the behavior of the material. Usually n is equal to 1, 2, or 3. As with the Mooney-Rivlin model the components of the stress tensor are determined by substituting eq. (3.6) into eq. (3.3) and performing the necessary differentiations.
Computer simulation o f thermoforming
85
Again the stress normal to the membrane surface is assumed to be negligible. Because the Ogden model is given in terms of the principal stretches instead of the invariants, 11 and I2, the physical meaning of the resulting stress-strain relations are much easier to determine.
3.3.2.2. Viseo-elastic models While non-linear elastic models effectively describe the material response under certain conditions, they must be applied with caution in actual thermoforming situations since they neglect viscous effects. For example, for relatively slow thermoforming viscoelastic effects have been found to be extremely important [32]. Hylton gives several examples of how the thermoformability of a given resin may be assessed on the basis of several visco-elastic properties. Perhaps the first finite element model to take visco-elastic effects into account is that given by Kouba et al. [19]. In their formulation the stress-strain data at different strain rates is fitted to a K-BKZ [33] constitutive equation modified by the inclusion of a Wagner damping function. The constitutive equation used is of the integral type and is given by t
s-
f
m ( t - t')h(I1,/2)B(t, t') dt'
(3.7)
where t' is the previous time, t is the current time, B(t, t') is the Finger strain tensor (left Cauchy-Green deformation tensor i.e. C -1) and m ( t - t') and h(I1,12) are the memory and damping functions, respectively. The damping function is of the form proposed by Wagner and Demarmels [34], and is written as 1
h(I1, 12) -
1 + av/(I 1 -
(3.8) 3 ) ( / 2 - 3)
where a is a material parameter and 11 and I2 are invariants of the Finger tensor B. The memory function which is related to the relaxation spectrum is given by (t--tt)
m ( t - t ' ) - Z ai e
(3.9)
ri
where ri are the relaxation times and a i are material constants and i is the number of relaxation processes considered. Assuming that pressure is applied and the deformation of the sheet starts at time t - 0 the stress in the two principal directions (i -- 1, 2) tangent to the surface of the sheet is given by t
S(t) - f m(t - t')h(I1, I2)[LZ(t, t')
-
LZ(t, t')] dt'
0
(3.10)
0
4- h(t)[LZ(t) - LZ(t)] f --00
m ( t - t') dt'
86
B.L. Koziey et al.
where Li(t, t') is the stretch ratio in the i th principal direction at time t related to time t', and L3(t, t') is the stretch ratio perpendicular to the sheet surface at time t related to t'. Temperature effects have also been included in the model because the model constants are a function of the temperature. Another approach to the inclusion of viscous effects in thermoforming is that presented by Vantal et al. [35]. They employ an approach similar to that used in metal forming. For deformation of the solid polymer under the glass transition temperature a visco-elasto-plastic constitutive relation of the form
-- kp(T)(g, e)
(3.11)
is used. Quantities 8, g and ~ are the effective stress, effective strain and effective strain rate, respectively, The temperature-dependence of the material response is included through the function kp(T). Beyond the glass transition temperature the rubbery polymer is modeled using a phenomenological visco-elastic constitutive relation. The material parameters were determined by fitting the constitutive model to uniaxial tensile data obtained for a wide range of temperatures and strain rates. In contrast to the other constitutive models described above, an updated Lagrangian finite element formulation is required since the constitutive relation is valid for small strains only.
3.3.3. Thermoforming simulation examples A finite element software package capable of modeling fully 3-D thermoforming, with or without plug assistance, has been developed and tested at McMaster University [18,36-38]. Extensive comparisons between predicted and experimental thickness distributions for both straight and plug-assisted thermoforming have been made which has established the validity of the finite element model. Experimental data on uniaxial or biaxial testing of polymers is scarce, especially at strain rates and temperatures that are within the ranges found in the thermoforming process. Nevertheless successful simulations have been carried out using both simple and complex mold geometries. For simple shallow mold geometries simulations using the non-linear elastic Ogden model are very accurate. A simulation of the vacuum forming of a simple dome-like automotive fuel tank component was performed using both the Ogden model and the visco-elastic K-BKZ model. The thickness distributions along a cut through the dome predicted by both models are plotted along with the actual thickness distribution in fig. 3.3. There is good agreement between the experimental results and both the Ogden and K-BKZ predictions. While the Ogden model is best suited for the simulation of straight thermoforming into shallow simple molds, the K-BKZ model is required when the simulation includes deep-drawn forming, complex mold geometry or plug assistance. The plug-assisted thermoforming simulation of a sheet into a complex mold was performed. The mold has a volume of about 22 liters and is used to form electronic device casings. A finite element mesh consisting of 1,536 elements was used to discretize the sheet which had an initial thickness of 6.35 mm (0.25 in.). The simulation was performed using both the Ogden and K-BKZ models. The K-BKZ model
Computer simulation of thermoforming
87
Fig. 3.3. Comparison of predicted and experimental final thickness distribution for automotive fuel tank component.
was fitted to material stress-strain data obtained for strain rates ranging from 0.01 s-1 to 10 s-1. The thickness distribution predicted using both material models is plotted in fig. 3.4, along with the experimental values for the cutting plane shown in the figure.
Fig. 3.4. Comparison of predicted and experimental final thickness distribution for film scanner casing.
88
B.L. Koziey et al.
The distribution predicted by the Ogden model is seen to be in poor agreement with the experimental data. However, the thickness distribution predicted by the KBKZ model is in very good agreement with the experimental distribution. This example clearly illustrates that the choice of material model (non-linear elastic versus visco-elastic) must be done very carefully if reliable predictions of the thickness distribution are to be obtained. 3.4. Concluding remarks A "state-of-the-art" review of the application of the finite element method to thermoforming simulation has been given. In general, the currently available models provide a rational means of mold design and can also aid in the optimization of the final resin distribution and the minimization of peripheral waste. While the existing models are capable of providing good predictions of the final part thickness, care must be taken in the selection of the material model used. Non-linear elastic models such as the Ogden model are attractive in their simplicity in comparison to viscoelastic models such as the K-BKZ model, but typically only provide reliable prediction for straight thermoforming (no mechanical assisted sheet stretching) into shallow simple molds. Future work should be targeted towards the development of less complex viscoelastic material models, inclusion of time-dependent thermal effects, and slippage of the sheet along the plug surface. In addition, more experimental data on uniaxial and biaxial stretching of polymers needs to be established at strain rates and temperatures typically experienced in the thermoforming process. References [1] [2] [3] [4]
Throne, J.L., Thermoforming, Hanser Publishers, New York, 1987. Tadmor, Z. & Gogos C.G., Principles of Polymer Processing, John Wiley & Sons, New York, 1979. Birley, A.W., Haworth B. & Batchelor J., Physics of Plastics, Hanser Publishers, Munich, 1991. Vlachopoulos, J. & Mitsoulis E., Fluid Flow and Heat Transfer in Calendering, in Transport Phenomena in Polymeric Systems, Ellis Horwood, Chichester, 1989. [5] Vlachopoulos, J., Calendering, in Concise Encyclopedia of Polymer Processing and Applications, Pergamon Press, Oxford, 1992. [6] Vlachopoulos, J., Silvi N. & Vlcek J., POLYCAD| A Finite Element Package for Molten Polymer Flow, in Applications of Computer Modeling for Extrusion and Other Continuous Polymer Processes, Hanser Publishers, Munich, 1992. [7] Vlcek, J., Perdikoulas J. & Vlachopoulos J., Extrusion Die Flow Simulation and Design with FLATCAD, COEXCAD and SPIRALCAD, in Applications of Computer Modeling for Extrusion and Other Continuous Polymer Processes, Hanser Publishers, Munich, 1992. [8] Zamani, N.G., Watt D.F. & Esteghamatian, M., Status of the Finite Element Method in the Thermoforming Process. Int. J. Num. Meth. Eng., 28 (1989) pp. 2681. [9] Oden, J.T., Finite Elements of Non-linear Continua, McGraw-Hill, New York, 1972. [10] Bathe, K.J., Finite Element Procedures in Engineering Analysis, Prentice Hall, Englewood Cliffs, NJ, 1982. [11] Zienkiewicz, O.C. & Taylor R.L., The Finite Element Method, Volume 1: Basic Formulation and Linear Problems, McGraw-Hill Book Company, London, 1988.
Computer simulation of thermoforming
89
[12] Zienkiewicz, O.C. & Taylor R.L., The Finite Element Method, Volume 2: Solid and Fluid Mechanics Dynamics and Non-linearity, McGraw-Hill Book Company, London, 1991. [13] Allard, R., Charrier J.M., Ghosh A., Marangou M., Ryan M. E., Shrivastava S. & Wu R., An Engineering Study of the Thermoforming Process: Experimental and Theoretical Consideration. J. Polym. Eng., 6 (1986) pp. 363. [14] Warby, M.K. & Whiteman J.R., Finite Element Model of Viscoelastic Membrane Deformation. Comput. Meth. Appl. Mech. Eng., 68 (1988) pp. 33. [15] Nied, H.F., Taylor C.A. & deLorenzi H.G., Three-Dimensional Finite Element Simulation of Thermoforming. Polym. Eng. Sci., 30 (1990) pp. 1314. [16] deLorenzi, H.G. & Nied H.F., Finite Element Simulation of Thermoforming and Blowmolding. Modeling of Polymer Processing: Recent Developments, Isayer, A.I. (ed.) Munich, 1991, pp. 117. [17] Taylor, C.A., deLorenzi H.G. & Kazomer D.O., Experimental and Numerical Investigations of Vacuum-Forming Processes. Polym. Eng. Sci., 32 (1992) pp. 1163. [18] Kouba, K., Bartos O. & Vlachopoulos J., Computer Simulation of Thermoforming in Complex Shapes. Polym. Eng. Sci., 32 (1992) pp. 699. [19] Kouba, K., Ghafur M.O., Vlachopoulos J. & Haessly W. P., Some New Results in Modelling of Thermoforming. SPE Tech. Papers, 52 (1994) pp. 850. [20] Mooney, M., A Theory of Large Elastic Deformation. J. Appl. Phys., 11 (1940), pp. 582. [21] Ogden, R.W., Large Deformation Isotropic Elasticity of Theory and Experiments for Incompressible Rubberlike Solids. Proc. R. Soc. Lond., A326 (1972) pp. 565. [22] Song, W.N., Mirza F.A. & Vlachopoulos J., Finite Element Analysis of Inflation of VacuumForming Processes. J. Rheol., 35 (1991) pp. 93. [23] Song, W.N., Mirza F.A. & Vlachopoulos J., Finite Element Simulation of Plug-Assist Forming. Int. Polym. Proc., 3 (1992) pp. 248. [24] Igl, S.A. & Osswald T.A., A Study of the Thermoformability of Wood Fibre Filled Polyolefin Composites. SPE Tech. Papers, 50 (1992) pp. 122. [25] Treloar, L.R.G., The Mechanics of Rubber Elasticity. Proc. R. Soc. Lond., A351 (1976) pp. 301. [26] Schmidt, L.R. & Carley J.F., Biaxial Stretching of Heat-Softened Plastic Sheets Using an Inflation Technique. Int. J. Eng. Sci., 13 (1975a) pp. 563. [27] Schmidt, L.R. & Carley J.F., Biaxial Stretching of Heat-Softened Plastics Sheets: Experiments and Results. Polym. Eng. Sci., 15 (1975b) pp. 51. [28] Ward, I.M., Mechanical Properties of Solid Polymers, John Wiley & Sons, New York, 1983. [29] Green, A.D. & Zema W., Theoretical Elasticity, Oxford University Press, New York, 1954. [30] Green, A.D. & Adkins J.E., Large Elastic Deformations, Oxford University Press, New York, 1960. [31] Eringen, A.C., Nonlinear Theory of Continuous Media, McGraw-Hill, New York, 1962. [32] Hylton, D., Laboratory Techniques for Predicting Material Thermoformability: A Review. SPE Tech. Papers, 49 (1991) pp. 580. [33] Tanner, R.I., Engineering Rheology, Oxford University Press, New York, 1985. [34] Wagner, M.H. & Demarmels A., A Constitutive Analysis of Extensional Flows of Polyisobutylene. J. Rheol., 34 (1990) pp. 943. [35] Vantal, M.H., Bellet M., Monasse B., Jammet J.C. & Andro R., PPS Tech. Papers, l0 (1994) pp. 317. [36] Kouba, K., Ghafur M.O. & Vlachopoulos J., Computer Modelling of Blow Molding. SPE Tech. Papers, 51 (1993)pp. 1861. [37] Kouba, K. & Vlachopoulos J., The Role of Rheology in Thermoforming Process: Experimental and Theoretical Consideration. SPE Tech. Papers, 50 (1992) pp. 114. [38] Vlachopoulos, J., Kouba K. & Ghafur M.O., The Role of Rheology in Thermoforming and Blow Molding, Fourth European Rheology Conference, Seville, Spain, 1994.
This . Page Intentionally Left Blank
Composite Sheet Forming edited by D. Bhattacharyya 9 Elsevier Science B.V. All rights reserved.
Chapter 4
Thermoforming of Continuous Fibre~Thermoplastic Composite Sheets K. F R I E D R I C H 1, M. H O U 2 and J. K R E B S 1 1Institute for Composite Materials Ltd. (IVW), University of Kaiserslautern, 67663 Kaiserslautern, Germany," 2Centrefor Advanced Materials Technology, Department of Mechanical Engineering, University of Sydney, Sydney, NSW 2006, Australia
Contents Abstract 92 4.1. Introduction 92 4.2. Experimental details and procedures 96 4.2.1. Materials employed for stamp and diaphragm forming 96 4.2.2. Preparation of pre-consolidated laminates 97 4.3. 2-D stamp forming 100 4.3.1. General remarks 100 4.3.2. Experimental details 102 4.3.3. Description of stamping process 104 4.3.4. Characterisation methods for thermoformed components 105 4.3.4.1. Microscopy 105 4.3.4.2. Characterisation of in-plane fibre movement 106 4.3.4.3. Thermal analysis 106 4.3.5. Results and discussion 107 4.3.5.1. Determination of preheating time 107 4.3.5.2. The forming temperature 110 4.3.5.3. Correlation between stamping velocity and stamping pressure 4.3.5.4. Effect of forming condition on part geometry 119 4.3.5.5. Thermoanalysis 130 4.3.5.6. Fibre movement studies 133 4.3.6. Optimised processing window for 2-D stamp forming 135 4.4. 3-D stamp forming 137 4.4.1. General remarks 137 4.4.2. Set-up of 3-D stamp forming device 138 4.4.3. Experimental procedure 139 4.4.4. Results and discussion 140 4.4.4.1. Stamp forming mechanisms 140 4.4.4.2. Stamp forming of GF fabric/PEI laminates 141 4.4.4.3. Stamp forming of UD GF/PP laminates 143 4.4.5. Recommendations for 3D stamp forming 145 4.5. 3-D diaphragm forming of GF/PP laminates 146 91
115
92
K. Friedrich et al.
4.5.1. General remarks 146 4.5.2. Experimental procedure 147 4.5.3. Assessmentand characterisation of thermoformed parts 148 4.5.3.1. Large strain analysis technique 148 4.5.3.2. Occurrence of defects and thickness variations in diaphragm formed parts 150 4.5.4. Variation of forming parameters and rating of part quality 152 4.5.4.1. The forming temperature 153 4.5.4.2. The forming ratio 154 4.5.4.3. The forming pressure 156 4.5.4.4. The forming velocity 156 4.5.4.5. The laminate thickness and lay-up 157 4.5.5. Conclusions and recommendations 157 4.6. Summary 159 Acknowledgements 160 References 160 Abstract Continuous fibre-reinforced thermoplastic polymers are a relatively young group of engineering materials compared with their thermosetting counterparts. However, due to their outstanding mechanical and thermal properties these materials are becoming increasingly attractive not only for aerospace and automotive applications. In order to produce defect-free components it is essential to gain a fundamental understanding of the effects of processing conditions on the structure and morphology of the resultant composite component. Only if the material's behaviour under the particular processing conditions is fully understood can the processing parameters be set in such a manner, that the desired microstructure and mechanical performance of the resulting component can be achieved. When forming continuous fibre-reinforced materials instabilities, such as wrinkles and buckles, may occur. In the example of the 2-D, 3-D and the diaphragm thermoforming technique it is demonstrated how the processing conditions can be optimised by individually investigating the parameters mainly governing the properties of the finished component ultimately enabling the production of defect-free parts. 4.1. Introduction Continuous fibre-reinforced thermoplastic polymers are still a relatively young group among the engineering materials compared with their thermosetting counterparts. However, due to their advantageous properties such as good thermal stability, high toughness/damage tolerance, infinite shelf-life and ease of processing, these materials are becoming increasingly attractive to various industrial sectors. In particular applications not only in the aerospace and automotive field but also in branches such as the medical, environmental and recreational industry represent potential markets. In order to exploit the advantageous features of continuous fibre-reinforced thermoplastic composites for a large array of industrial applications and products,
Thermoforming of cont&uousfibre~thermoplastic composite sheets
93
several manufacturing methods have been developed over the last decade [1]. Utilising related processes known from thermosetting composites and adapting sheet forming techniques typical of those used with metallic materials, fabrication techniques, such as compression moulding, tape winding, thermoforming, joining and pultrusion have become available (fig. 4.1). However, the introduction of advanced thermoplastic composites has also led to novel requirements being imposed on processing techniques for manufacture of high-quality intermediates. Unlike thermosets, which are usually compounded at the moulding site, fibre-reinforced thermoplastics have to be supplied in a variety of different ready-to-use intermediates in order to match the requirements of the various production techniques [2]. Embedding the reinforcements into high-viscosity thermoplastic matrices is still a demanding task. Many approaches were necessary in order to overcome the difficulties of impregnation enabling the production of intermediate material forms such as film stacked prepregs (pre-impregnated materials), commingled fibres,
Fig. 4.1. Processingwith thermoplasticcomposites.
94
K. Friedrich et al.
pultruded bands and powder impregnated bundles which are commonly used in contemporary thermoplastic manufacturing technology (fig. 4.2) [3]. In order to produce good quality parts it is necessary to initially gain a fundamental understanding of the effects of processing conditions on the structure and morphology of the resultant composite component [4--6] (fig. 4.3). Only if the material's behaviour under the particular processing conditions is fully understood, can the processing parameter be set in such a manner that the desired microstructure and mechanical performance of the laminate can be achieved. In this chapter two thermoforming techniques, stamp forming and diaphragm forming, are investigated with regard to their potential for producing defect-free
Commingled Fibers
Film Stacking
I lll
~-~ Reinforcing Fibers
Fiber Woven Fabric
Polymer Fibers ~ ' - u I u i u i u~ Polymer Films
Powder Impregnated Bundles
Pultruded Band
Fiber Bundle
~
Fiber
Polymer Powder
Polymer
olymer Sheath
Fig. 4.2. Intermediate material forms for thermoplastic composites.
Intermediate Material
Form
H
Processing Method
a.) Commingled Yarn
a.) Compression Molding
b.) Powder
b.) Tape
Impregnated
Fibers
c.) Melt Impr, Tapes
Winding
c,) Stamp Forming
H
Processing Parameters
m,.,cro,u.,r,uo,H
Mechanical
of Bulk Composite
Performance of Laminate
a.) Interlaminar a.) Temperature a.) Morphology Fracture of Crystalline b.) Pressure Polymer Matrix Toughness b.) Materials c,) Time b.) Alignment Stiffness of Fibers and Strength d.) Cooling c.) Formation of Voids [
,
.....
I
No
I
I
Fig. 4.3. Methodology for fundamental studies on processing properties of thermoplastic composites.
Thermoforming of conth~uousfibre/thermoplastic composite sheets
95
components from continuous fibre-reinforced thermoplastic prepreg materials. The particular interest in stamp forming stems from its obvious suitability for mass producing single and double curvatured parts at considerable low cycle times. Diaphragm forming on the other hand is very unlikely to match the productivity of stamp forming; however, when it comes to producing very complex-shaped structures, this technique appears to be more suitable due to its capability to accommodate inter-ply shear induced laminate thickening. Here, superplastic aluminium diaphragms like Supral TM* were originally employed for vacuum-bagging hightemperature fibre/matrix systems such as CF/PEEK (APC-2 TMt, AS4) in autoclaves. Due to the pronounced strain-rate sensitivity, consequently resulting in high cycle times, the fairly restricted stretchability and the high temperatures required for achieving maximum elongation, lately most emphasis has been placed on the use of polymeric diaphragms such as Upilex TM* [1,7-9]. Since polyimid diaphragms are not strain-rate sensitive, forming can be completed in a matter of minutes in contrast to approximately 20 minutes that are required for superplastic aluminium diaphragms. It has to be noted, however, that due to the thermal properties of polyimid diaphragms they are only suited for processing composites containing high melting temperature matrices such as PEEK (poly ether ether ketone) and PEKK (poly ether ketone ketone). As a consequence, when looking into industry branches where attributes such as high volume production, cycle times in the order of seconds, low material costs and automation are of decisive significance, these materials, despite their superior properties, will have difficulty in asserting themselves against the traditional engineering materials which are still dominating the market. According to recent trends in the composites industry, structural materials such as glass-fibre-reinforced polypropylene and polyamide do have the best future prospects for substituting metallic materials in markets such as the environmental sector where there are tremendous opportunities for glass-fibre-reinforced thermoplastics sewage pipes, scrubbers and tanks [10]. Also in the automotive industry where polypropylene is already well established as non-reinforced material the number of glass-fibre-reinforced components is continuously growing. Today, parts such as noise shields, bumper carriers, compartment capsulations and seat shells are made from glass-mat-reinforced thermoplastics (GMT) in order to name only a few [11]. An expansion to continuous glass fibre-reinforced polypropylene structures, therefore, appears to be a more than sensible venture. One of the most recent additions in the group of structural composite materials are Plytron TM~ and Tepex TMw Fundamental studies on the formability and the resulting part properties of this material, as well as mechanical properties and environmental resistance have already been conducted by a number of research groups. However, there is still far more work necessary in order to make thermoforming of such *SupralT M is an Alcan Registered Trademark. tAPC_2TMis a ICI Ltd. Registered Trademark. SUpilexT M is a UBE Ind. Registered Trademark. ~PlytronT M is an ICI Ltd. Registered Trademark. w T M is a DuPont Registered Trademark.
96
K. Friedrich et al.
materials become a repeatable and cost-effective fabrication technique capable of producing accurately predictable finished part properties at acceptable cycle times. Employing a number of differently reinforced matrices, unidirectional and fabric, and different types of reinforcing fibres, carbon and glass, the intention of this chapter is to outline the durability and limitations of both stamp and diaphragm forming. It addresses aspects such as flow processes occurring during thermoforming, consolidation quality and achievable structural properties of the resulting components. Moreover, the occurrence of instabilities in the finished components such as wrinkling and buckling in both processes is investigated and illustrated with the aim of creating a complete picture of their potentials and limitations.
4.2. Experimental details and procedures 4.2.1. Materials employed for stamp and diaphragm forming This section intends to give an introduction to the structural and physical properties of the materials employed for the investigations into stamp and diaphragm forming. Furthermore, the procedures followed for pre-consolidating laminates for later usage in the forming experiments is described and illustrated since it is felt that this step has a significant influence on the material's behaviour under thermoforming conditions and the resulting component properties. The following section also provides an introduction to all prepreg materials employed for the subsequent series of experiments, outlining their physical and thermal properties. The most important properties are summarised in table 4.1. (a) Continuous glass fibre (GF) reinforced thermoplastic composite called Plytron | with a polypropylene (PP) matrix, by ICI Ltd., UK. The nominal glass fibre content of this material is 60 wt. % and 35 vol. % glass/polypropylene. The material was supplied as a tape with a width of 240 mm and a nominal thickness of 0.47 mm. TABLE 4.1 List of materials employed for thermoforming experiments Advanced thermoplastic composites (abbreviations)
Melt temp. (~ Glass trans, temp. (~ Fibre volume fraction (%) Material form Manufacturer 2-D forming 3-D froming
GF/PP
CF/PP
GF/PP
CF/PA12 CF/PEEK GF/PEI
145-170 -20 35 Prepreg ICI Ltd. UK
163
163
176
334
20 Prepreg ICI Ltd. UK
33 Prepreg BASF Germany
40 60 Plate Enichem Italy
60 Plate Enichem Italy
9
210 50 Prepreg Ten Cate Holland
Thermoforming of continuousfibre~thermoplastic composite sheets
97
(b) Pultruded continuous carbon fibre (CF) polypropylene (PP)-tape, with a nominal thickness of 0.50 mm and a nominal fibre content of 33 vol. % carbon/ polypropylene, manufactured by ICI Ltd., UK. (c) Pultruded continuous glass fibre (GF) polypropylene (PP)-tape, with a nominal thickness of 0.50 mm and a nominal fibre content of 20 vol. % glass/polypropylene, manufactured by BASF AG, Germany. (d) Continuous carbon-fibre-reinforced pre-consolidated laminates with a polyamide (PA-12) and a polyetheretherketone (PEEK) matrix manufactured by Enichem, Italy. The nominal fibre content of these materials is 40 vol. % and 60 vol. % carbon/polyamide 12 and carbon/polyetheretherketone respectively. The uni-directional (UD) laminates with a nominal thickness of 3.2 mm were made from powder-impregnated fibre bundles. (e) Glass fibre fabric (GF) reinforced amorphous polyetherimide (PEI) manufactured by Ten Cate, The Netherlands. Here, the fibre content is 50 vol. % glass/ polyetherimide with a nominal tape thickness of 0.80 mm. The weave style of the glass fabric was 8 H satin and is illustrated in fig. 4.4. 4.2.2. Preparation of pre-consolidated laminates
An integral part of all forming processes is the consolidation of flat laminates which is either accomplished during forming (in-situ processing) or carried out prior to the actual thermoforming process. Since the properties of the moulding are essentially dependent upon the quality of the lamination, it is important to thoroughly define and control the conditions under which well consolidated material may be obtained. In principle, lamination involves two processes: (a) obtaining autoadhesion between the plies and (b) removing that which lies between them (air or water vapour) [12]. This can be achieved by using either pressure in order to dissolve the air into the melt or vacuum to extract it. For the 2-D and 3-D stamp forming experiments pre-consolidated sheets (100 x 160 mm and 128 x 128 mm) were prepared by pressurising a loose stack of plies with a predetermined stacking sequence in between two heated platens. The unidirectional and quasi-isotropic sheets with a [0~ [0~176176 and [0~176 s [13] stacking sequence were made from CF/PP and GF/PP (BASF) prepregs according to the
Fig. 4.4. Woven structure of 8-H satin glass fabric in GF/PEI composite.
98
K. Friedrich et al.
following procedure. First, a steel mould filled with several layers of prepreg material is placed in a heatable press. The stacked pile of plies is then preheated in the absence of pressure until the matrix has reached its molten state. Consolidation is achieved by applying external pressure for about 5-10 min. Finally, the mould is cooled below the melt temperature of the matrix whilst maintaining the applied pressure in order to prevent the occurrence of voids within the laminate. The consolidation temperature and pressure have to be carefully monitored throughout this process since too high a temperature and/or pressure can lead to undesired fibre misalignment caused by excessive matrix flow and fibre migration. However, on the other hand, if the temperature and pressure are set too low the resulting laminates are likely to contain high void content and poor inter-ply bonding. The resulting sheets employed within this study exhibited a thickness of 2.8-3.0 mm. A simple but effective method for characterising the movement of the reinforcements during forming is to embed tracer wires made from material that is not transparent to X-rays into the surfaces layer of a pre-consolidated laminate (e.g. copper wires). The motion of the wires during stamp forming can then be detected by X-ray analysis techniques or usage of powerful light sources for composites with transparent or opaque matrices. The technique utilised for fabricating pre-consolidated laminates with embedded copper tracer wires is illustrated in fig. 4.5. First, the copper wires are mounted onto a metal frame with a uniform lateral distance between them. Then the copper wires are pressed onto the surface of a prepreg ply using a hot press set to the melting temperature of the individual matrix in the ply. The plies with integrated copper wires thus obtained are then used for preparing sheets for subsequent fibre motion measurements. For the stamp forming experiments described here, blanks were cut to size, as shown in fig. 4.6, where L denotes the length, B the width and do the original thickness of the laminate. In order to measure the temperature profile of the heated pre-consolidated sheets during stamp forming, NiCr-Ni thermocouples were embedded into the centre layer of several laminates. An alternative method that may be employed for the production of pre-consolidated laminates is depicted in fig. 4.7. For implementing the diaphragm forming
Fig. 4.5. Schematic diagram of manufacturing pre-consolidated laminate with embraced Cu trace wires.
Thermoforming of continuousfibre/thermoplastic composite sheets
99
Fig. 4.6. Definition of sample cut from GF fabric/PEI laminate.
Metal Frame with Gasket u,apnra~m Top Plate
~(Alumini
;
j
/
~g~'~
m)
, ~ ~ O v e n Bag #2 , Stacked ~Prepreg Plies ~ M e t a l Strip ~ O v e n Bag #1 Vacuum Table (Aluminium) Outlet to Vacuum Pump
Fig. 4.7. Preconsolidation device for diaphragm forming experiments.
experiments it was decided to use vacuum rather than pressure for pre-consolidating rectangular flat sheets with different lay-ups and thicknesses. In order to consolidate a multi-ply sheet a completely uncompacted stack of plies is placed on a vacuum table. Oven bags (Melinex Type S [14]) covering the plies prevent the material from sticking to the aluminium platens and metal strips surrounding the plies during consolidation. Applying a vacuum pressure of about - 2 0 kPa the stack of plies is heated up in an oven to the matrix's melt temperature where it dwells for about 15 minutes. In the case of Plytron, the cooling rate which basically determines the
1O0
K. Friedrich et al.
extend of crystal growth in the semi-crystalline polypropylene matrix should be greater than 1~ since otherwise too high a level of crystallinity is achieved, resulting in a low fracture toughness [12].
4.3. 2-D stamp forming 4.3.1. General remarks
Thermoplastic polymers can undergo a reversible phase change from solid to liquid, thereby enabling the development of shaping and joining methods analogous to those for conventional metallic materials. When transferring a flat, continuousfibre-reinforced laminate into a 3-D shaped component a number of different deformation mechanism governing the forming behaviour of this material have to be taken into account. Unlike the monolithic metallic sheet, continuous fibre-reinforced thermoplastic (CFRT) materials are virtually inextensible in the direction of the reinforcement. For these material systems, the dominant mode of deformation, parallel to the fibres, during sheet forming is therefore shearing within the individual plies and between them, namely intra- and inter-ply shear. Additional mechanisms that occur when transferring a flat multi-ply sheet into a double curvature formed component are resin percolation through and along the layers of the reinforcing fibres, resin flow transverse to the fibres and rotation of adjacent plies relative to one another [15-19]. A schematic diagram of the deformation modes in the increasing order of shape complexity and correlated flow mechanisms shown in fig. 4.8 can be described as follows. (a) Resin percolation is fundamental to all flow processes and occurs to some extent in all types of fabrications. It is the flow of polymer matrix through and along the layers of the reinforcing fibres. This process allows layers of prepreg to be bonded together to form one sheet. Fritzer and J~iger studied the flow behaviour of matrix materials in order to optimise the processing parameters such as pressure and temperature leading to a homogeneous distribution of the matrix in the composite [20-22]. (b) Transverse flow is the process by which a prepreg spreads out to accommodate local pressure variations during forming processes. It is responsible for apparent stretching that can occur in a unidirectional laminate in perpendicular direction of the reinforcements [23]. A small amount of transverse flow is observed during any forming process at elevated forming temperatures caused by local pressure gradients that arise from small variations in the laminate thickness and mould clearances [13,24]. Transverse flow can also result from shear stresses developing between the thermoplastic material and the forming tool surface. (c) Inter-ply slip is a relative shear movement of two adjacent laminate layers. In this case the polymer matrix acts as a lubricant between neighbouring plies. When a laminate is formed onto a curved surface it has to deform in such a manner that inter-ply slip can account for the gradual change in shape. If this process is inhibited fibre wrinkling and buckling are normally the result [25-27].
Thermoforming of continuous fibre/thermoplastic composite sheets
101
Fig. 4.8. Deformation modes and flow mechanisms of continuous fibre-reinforced thermoplastic materials. [1].
(d) Intra-ply shear is needed when a shearing strain occurs in the plane of the laminate, thus allowing part conformity to complex curvature geometry. Theoretically, there is no limit to the amount of shear deformation in unidirectional laminates. Fabrics, by contrast, are usually interlocked at fibre crossover points, limiting the shear strain to the locking angle of the unit cell (trellis angle) [281. (e) Inter-laminar rotation is required for forming multi-ply laminates into double curvatured shapes. This shear action occurs in a thin "resin-rich layer" that forms at each laminate surface during consolidation due to resin migration. Most complex curvature parts require a change of initial fibre orientation between adjacent plies. For the production of 2-D and 3-D components the occurrence of inter- and intraply shearing processes is of particular interest. Only if the reinforcements can alter their orientation by shearing and rotating relative to one another during forming instabilities such as wrinkles and buckles can be prevented from occurring. Therefore, particular attention has to be devoted to these flow mechanisms in any thermoforming procedure for continuous fibre-reinforced thermoplastic composites.
102
K. Friedrich e t al.
4.3.2. Experimental details
In the series of 2-D stamp forming experiments described in the following subsections, the quality of the finished components made from fiat pre-consolidated laminates is evaluated by investigating the effect of the processing parameters such as pressure, temperature, cycle time, velocity, mould geometry and laminate architecture on the microscopic and macroscopic properties of the formed parts. For this series of experiments blanks made from CF/PP, GF/PP (BASF), CF/PA12, CF/PEEK and GF fabric/PEI were employed. The 2-D stamp forming experiments were conducted employing the matched metal die forming process as it is commonly known from sheet metal forming. For simplicity, the forming set-up was mounted into an universal testing machine that allowed closing velocities ranging from 1 to 1,000 mm/min. Forming was carried out under non-isothermal conditions, which means that the pre-consolidated laminates had to be pre-heated to processing temperature in a laboratory hand press prior to forming. Once the desired temperature was reached the laminates were then transferred into the press and formed immediately. In order to record the load conditions occurring during forming, an x - y recorder was connected to the press's pressure transducer. The alignment of the male and female moulds was realised by two pillars ensuring that both mould parts were kept aligned (fig. 4.9). The male mould was supported by two coil springs surrounding the pillars. The springs not only prevented possible damage to the pressure transducer that can occur at high
Fig. 4.9. Schematic diagram of angle mould for 2-D stamp forming.
Thermoforming of continuousfibre/thermoplastic composite sheets
103
loads but also allowed the moulds to open up automatically after each processing cycle, easing de-moulding and handling of the formed samples. In the forming series discussed in this section three pairs of right-angle vee-shaped moulds with three different bend-radii (2.5, 5.0 and 10.0 mm) were employed with a uniform clearance between male and female mould of 2.5 mm (fig. 4.10). The universal testing machine was operated as a load-controlled mechanical press under compression mode. The maximum applicable stamping pressure was controlled by pre-setting switch-off pressures. Figure 4.11 depicts the correlation of stamping pressure and stamping stroke versus time. Here, the solid line represents the load and the tinted line the stroke of the stamper. In order to form a part, the stamper was driven at a constant speed. Once it physically touches the pre-heated laminate forcing it into the cavity of the female mould, the load increased until the pre-set switchoff load was reached which immediately terminated the forming stroke. The forming
Fig. 4.11. Definition of processing parameters.
104
K. Friedrich et al.
durations thus obtained ranged from 4 to 20 s dependent on the stamping velocity (fig. 4.12). Due to inaccuracies in the press's control unit, reaching the switch-off load did not immediately lead to a halt of the stamper, but resulted in a swing-over effect which increased with increasing stamping speed. After the peak value was reached the compression pressure began to drop to an equilibrium pressure level which can be related to processes such as matrix flow, fibre migration and shrinkage of the laminate that occur upon cooling. An additional finding of this series of forming experiments was that the stacking sequence of the laminate also significantly affects the final stamping pressure. The effects of this phenomenon will be discussed in more detail in section 4.3.5.3.1. 4.3.3. Description o f stamping process
Generally, the deformation behaviour of thermoplastic composites are directly linked to their processing temperature. Amorphous polymers can be deformed when in their rubber-plastic state (above glass transition temperature Tg), whereas semi-crystalline polymers can only be deformed near or above their melting temperature. Therefore, pre-consolidated laminates produced as described in section 4.2.2 generally have to be subjected to some pre-heating procedure before deformation can take place. There are three different principles that may be utilised for preheating thermoplastic laminates: (i) conduction heating between two heated platens, (ii) infrared heating and (iii) forced convection in air or inert gas circulation ovens. In this part of the study contact heating plate were employed for heating pre-consolidated sheets because this method was found to relatively efficient on a laboratory scale [29]. The major drawback of this method, however, was found to be that the laminate may de-consolidate during heat-up, and the tendency of the molten matrix to stick to the contact surface of the heated platens. Therefore, in order to ease the 25 o 20 2: o,-~ ~9 ,__.~ 15
H
= O
E I-
\
g
10
.,-.,
5 0
200
400
600
Stamping velocity v [ mm/min ]
/
H ts~
Fig. 4.12. Closing time in relationship to stamping velocity.
h
v
800
Thermoforming of cont&uousfibre~thermoplastic compositesheets
105
handling of the heated sheets it is advisable to sandwich them between two polymeric diaphragms, i.e. polyimide films such as Kapton 200 HN. An advantageous side effect of this measure is that it normally enhances the quality of the surface finish of the finished components and it also reduces the cooling rate of the heated sheets during forming. This way the total duration at which the laminate can be deformed is significantly extended. In order to form a part, the sheets were pre-heated to processing temperature, then transferred into the stamping device and formed. Transferring should not exceed a few seconds so that the laminate retains its formability. During stamping the laminate is cooled below its glass transition temperature or melting temperature through the direct contact with the cold metal moulds. This means that de-moulding can normally take place directly after forming is accomplished. The geometry of a fiat laminate and a stamped bend is depicted in fig. 4.13, where L denotes the length, B the width, 0 the final angle of the stamped bend, d the final laminate thickness, and Ad the reduction in thickness relative to the original thickness do. Two different types of blanks (a) B = 15, L = 80 and (b) B = 60, L = 80 were used for these experiments, where the latter had copper wires embedded for subsequent X-ray analysis procedures.
4.3.4. Character&athgn methods for thermoformed components 4.3.4.1. Microscopy Optical microscopy is a suitable and inexpensive method for examining the fibre arrangement and impregnation quality of polished cross-sections of stamped samples. For this purpose, specimens cut from stamped vee-bend components L o
_-o
l
"
!
(a)
Length Direction
(b) ~
90
~ -
Fig. 4.13. Sample geometry and its definition.
/
106
K. Friedrich et al.
were embedded in epoxy resin and polished with 180, 500, 800 and 1200 sand paper, followed by polishing with 1 ~tm AL203 paste. Photographs were taken from three sections in one specimen, i.e. at both ends and the bend region. 4.3.4.2. Characterisation o f in-plane fibre movement
A qualitative study investigating the in-plane fibre movement in stamp-formed components was implemented by using X-ray analysis techniques on specimens with embedded copper tracer wires. X-rays (produced by RBVII/TYK9B, Rich, Seiteut & Co.) travel through the formed sample sensitising a film (AGFAGEVAERT D4) placed behind the sample (fig. 4.14). Due to the higher absorption of X-rays of the copper wires, these wires appear as dark lines on the film. In order to evaluate the distortion of copper wires, the lateral distance between adjacent wires has to be measured. The histogram of copper wires at different distances compared with the corresponding original alignment (standardised distance between adjacent copper wires in this experiment: 2.5 mm) indirectly indicates the magnitude of fibre migration. 4.3.4.3. Thermal analysis
The crystallinity of thermoplastic polymers mainly depends on their thermal history experienced during forming. In order to study the effect of processing conditions on the morphological properties of the matrix materials, DSC (Differential Scanning Calorimetry) is a suitable method for determining the degree of crystallinity of polymeric matrices before and after forming. For this reason, test samples (weight ~ 10 g) were cut from the stamp formed parts and heated at a rate of 10~ Principally, the crystallinity of a polymer is determined by integration of its DSC curve. The measured enthalpy AH is directly proportional to the degree of crystallinity of the matrix but also proportional to the matrix fraction in the sample. Therefore, after each DSC measurement the tested sample needs to be subjected to a TG-analysis (Thermal Gravimetry) in order to determine the pure matrix weight (WT~). With AHc as the degree of enthalpy for 100% crystallinity, the
X-ray
Film
Outer Surface
Inner Surface
Fig. 4.14. Schematicdiagram of X-ray equipment.
Thermoforming of continuousfibre~thermoplastic composite sheets
107
following equation can be applied for the calculation of the crystallinity of a polymer: C=
AH WDS C
Anc WTo
• 100 [%]
(4.3.1)
where C = crystallinity of a sample [%], W D S C - - sample weight for DSC-analysis [g], AH = enthalpy measured by DSC-analysis [J/g], WXG = matrix weight of the same measured by TG-analysis [g], and AHc =theoretical enthalpy for 100% crystallinity [J/g]. In order to acquire data for a theoretical calculation of the final angle reduction of vee-bent parts (section 4.3.5.4.3), the thermal expansion coefficients of pre-consolidated laminates along and perpendicular to the fibre direction have to be determined by TMA (Thermal Mechanical Analysis). The samples (5 • 6 • 6 mm 3) were cut from pre-consolidated plates with a diamond saw. It has to be noted that during the preparation of TMA samples the surfaces between detector and sample table has to be kept parallel. The heating rate in this study was set to 2~ with a load of 0.1 N applied to the detector which was equivalent to a pressure of 5.6 kPa. The measuring temperature range for the individual fibre/matrix system was determined by the melting temperature of the corresponding polymeric matrix.
4.3.5. Results and discussion 4.3.5.1. Determination of preheating time The contact heating method employed is a one-dimensional unsteady-state conduction procedure. Thermal conduction is an energy transportation through atomic and molecular interactions resulting from unequal temperature distributions. A simple heat transfer analysis can be used to obtain an estimate of the pre-heating time. Equation (4.3.2) describes the general three-dimensional thermal conduction problem, regarding the temperature as a function of position in space and time [30]: 8t = P-~e \~2x + ~
+ ~2z }
(4.3.2)
where T = plate temperature [~ t =time [s], X = thermal conductivity [Cal/ cm s ~ Cp = specific heat [Cal/g ~ and p = density [g/cm3]. Since the length and width of the pre-consolidated plates were much bigger than the thickness, it was assumed that the heat can only be conducted in the laminate's thickness direction. The heating process can therefore be reduced to an one-dimensional heating problem. The one-dimensional unsteady-state heat conduction model is illustrated schematically in fig. 4.15. Assuming that (a) the thickness of the two polymeric films is almost zero and therefore negligible and (b) the surfaces of the plates reached the pre-set heating temperature (Zheating) as soon as heating is initiated and retain this temperature throughout the process. The plate which had to be heated was of a thickness of 2x0 and an initial temperature of To. Then the differential equation for unsteady-state heat conduction in one direction is:
108
K. Friedrich et al.
Fig. 4.15. One-dimensional unsteady-state heat conduction model. ST_ 6t
k~ ( 8 2 T ~
-pc.
\-r
(4.3.3)
t > o, o < ~ < ~o
with the following initial and boundary conditions: dT ~=0, dt T -- Theating
x-0,
t>0
(4.3.4)
X - X0,
t> 0
T -- T o
O<.x<.xo
t -- 0
(4.3.5) (4.3.6)
Boundary condition (4.3.4) is symmetric to the middle plane of the plate (x = 0). Therefore, the temperature distribution is also symmetric to this plane and there is no energy flow through this plane. The analytical solution of eq. (4.3.3) can be written as: i-~176
Y= Z
r
[2i -- i)-~rr
cos
( 2 i - 1) 2 " x r x n
(4.3.7)
i=1 where
9
Y _~
rHeiz- T T H e i z - T O'
z
'
)~t ~ Cpp X 2'
~
n
~
x X0
In order to estimate the heating time two physical properties of the composite are needed, i.e. thermal conductivity ~. and specific heat Cp. The following equations are usually used for calculating these properties [31]: Cpc -- L ( ~ . f p f C f + ).mPmCm) Pc ~c-
Xm4U
[1 -- ~/~]/~'m "+-
1
(4.3.8)
(4.3.9)
Thermoforming of continuous fibre/thermoplastic composite sheets
109
Here, the indices m, f and r denote the matrix, fibre and composite respectively. The thermal properties of the materials used for the evaluation of the heating time are listed in table 4.2 [32-37]. Using eqs. (4.3.7), (4.3.8), (4.3.9) together with the data given in table 4.2, the temperature profile of the middle plane (x = 0) in relation to the heating time can be calculated. The time, at which the temperature of the middle plane reaches Theating is the estimated preheating time. Figure 4.16 illustrates the temperature profile of the middle plane of a CF/PP laminate as a function of heating time. For GF/PP material the heating plate was heated up to 180~ and the laminate had a thickness of 3.0 mm. In order for the middle plane to reach this temperature approximately 34 s were needed. The difference between the estimated and actually measured value was about 10 s. The reason for this discrepancy can be explained with the two polymeric Kapton films which were not accounted for in the estimation. Naturally, with increasing laminate thickness, extended heating times are needed in order to heating the middle ply of the laminate to the desired temperature (fig. 4.17). Preheating times estimated for different laminates are summarised in table 4.3. TABLE 4.2 Physical property of materials used Physical property Abbreviation
Thermal conductivity (cal/cm s ~
Heating capacity (cal/g ~
Density (g/cm 3)
CF GF PP PAl2 PEEK PEI
2.03 2.08 5.26 5.49 5.97 5.25
0.22 0.20 0.41 0.28 0.32 0.37
1.80 2.55 0.90 1.02 1.32 1.27
:3 "~
9
x x x x x x
250
L
~ ag
10- 2 10-3 10-4 10-4 10-4 10-4
T 'Heating
~J
...............
i
,
plate
-,,
q
|
i
i
{ ..............
i:i: ii:i:iiiiii.......... ;i loo i
O
I--
50
-
~ 4 -
~ .
[
~
0
10
.
.
Estimated data . data
20 Heating time [ s ]
Fig. 4.16. Heating temperature profile of CF/PP laminate.
30
j 40
110
K. Friedrich et al.
i /mHeating plate
350 --~ O ~
280 210
.~ "--" 140 E
Ill ..................i]............................................ i....................
70
~"
~ f .............................
.............................................
i
0 0
20
i......................
o o
,~
Zx
40
60
'mm' 00 "
a . a s
5.00
80
...........
1O0
Heating time [ s ] Fig. 4.17. Estimated heating time in relationship to laminate thickness.
TABLE 4.3 Estimated heating time Abbreviation
Theating
tcentral layer
(~
(s)
Fibre volume fraction (%)
Laminate thickness (mm)
CF/PP GF/PP
20 33
3.0 2.9
180
34 36
CF/PA12
40 60
3.2
220
24 16
CF/PEEK
60
3.2
380
18
GF fabric/PEI
50
2.6 3.9 5.0
280
28 62 103
4.3.5.2. The forming temperature One of the major problems in thermoforming processes is the determination of the temperature range within which a laminate can be successfully formed. A fairly simple but effective way of monitoring the temperature history in a laminate during forming under non-isothermal conditions is to embed a NiCr-Ni thermocouple into the laminate prior to forming (fig. 4.18). Naturally, this method is only feasible on a laboratory scale or in the preparation and adjusting phase for manufacturing a large batch of parts. In the following investigation a series of experiments are described in which the stamping velocity was varied from 500 mm/min down to a value at which the laminate could no longer be deformed. The temperature profile of CF/PP laminates as a function of the processing time was monitored and is illustrated in fig. 4.19. The
Thermoforming of continuous fibre/thermoplastic composite sheets
111
Hot laminate
/
----
NiCr-Ni
Thermocouple
Fig. 4.18. Temperature measurement during stamp forming.
200
i J
175 -,9
9
I ~
i .:
................................. ]- ........................................ ! ....................................................................................
'
I
!
i ......................................................................................
j
150
t
~
125 o
~.
75 5o
25
'
0
"J 0
' 10
, 20 Stamping
. . . . . 30
40
i 50
, 60
time [ s ]
Fig. 4.19. Temperature profile of CF/PP laminate during stamp forming.
upper linear bound along the black dots indicates the cooling rate of a laminate in an ambient environment which basically represents the condition where the heated laminate is not yet in contact with the cold surface of the tool. The temperature at which the cooling of the laminate starts dropping more rapidly (due to the tool/ laminate contact during closing) is defined as the stamping temperature. Its value raises with increasing stamping velocity. In two-dimensional forming such as vee-bending, inter-ply shear is one of the most important deformation mechanisms which allows the individual plies to slip relative to one another and thus prevents instabilities from occurring in the laminate [38]. In principle, inter-ply shear can be regarded as the result of a pressure/velocity gradient
112
K. Friedrich et al.
between adjacent plies of the laminate. However, if the stamping velocity is too low, the actual temperature of the laminate drops below a temperature level where interply slip can no longer occur (fig. 4.20). In this case, the shear stress acting on the plies does not exceed the shear yield stress of the matrix material, which ultimately results in fibre buckling at the inner face of the bend. In addition, fibre breakage can occur in the outer face. An example of the buckling phenomenon is represented in fig. 4.21, for which the forming temperature of the laminate was as low as 156~ When stamping [0~ and [0~176176 laminates fibre buckling can be observed at the inner face of the bend area. Stamping [0~176 laminates the velocity is still high enough to produce good quality samples. This result is related to the significant transverse intra-ply shear in the 90 ~ layers, for which a much lower yield shear stress 180
=
170
r Q.
E "" ~
~
=
160
0
150
E co
140
0
100
200
300
400
500
600
700
800
Stamping velocity [ mm/min ] Fig. 4.20. Effect of stamping velocity on stamping temperature of CF/PP laminate.
Fig. 4.21. Fibre buckling at inner bend section (CF/PP) laminate.
Thermoforming of continuousfibre~thermoplastic composite sheets
113
has to be exceeded. At stamping velocities in excess of 200 mm/min the stamping temperature of the laminates stays above 160~ This is sufficient for ensuring defectfree bend samples independent of the laminate's stacking sequences. Micrographs of polished cross-sections of the bend regions give clear evidence for the good quality of the stamp formed parts under these conditions (fig. 4.22). In this situation inter-ply slip between the individual plies of the laminate are clearly visible even at the far end of the bend samples (fig. 4.23). The surface finish of these parts can also be rated as
Fig. 4.22. Micrograph of the curved area of [0]6 CF/PP laminate.
Fig. 4.23. Inter-ply slip at the bend end of CF/PP laminate.
114
K. Friedrich et al.
satisfactory since no fibres have migrated to the surface during the forming operation. Increasing the stamping velocity, on the other hand, decreases the mould closing time, thus keeping the stamping temperature relatively high. When, in addition, the stamp pressure is set too high, large portions of matrix are squeezed into the outer range of the bend area (matrix migration) whereas the fibres accumulate in the inner bend region (fig. 4.24). The reason for this is that although the critical shear stress for inter-ply slip is exceeded locally, i.e. in the curved area, there is not enough time for this flow mechanism to take place at the two fiat ends of the vee-bend. Figure 4.25 schematically shows the possible fibre distributions after stamp forming that may be obtained with different forming temperatures. Another example of the effect of stamping temperature is given for the amorphous PEI matrix, reinforced with glass-fibre fabric. The glass transition temperature of PEI is 210~ If the temperature exceeds that level the GF fabric/PEI laminate
Fig. 4.24. Matrix migration at bend angle section of CF/PP laminate.
Fig. 4.25. Possible fibre distribution after stamp forming.
Thermoforming of continuous fibre/thermoplastic composite sheets
115
should be formable in the presence of an external load. A series of experiments shows, however, that the temperature for GF fabric/PEI laminates has to be clearly higher. The laminates had to be preheated to 280~ in order to achieve defect-free components. Figure 4.26 illustrates the temperature drop-off during stamp forming. The preheating temperature of 280~ results in a stamping temperature of the laminate of only 260~ when the stamping velocity amounts to 200 mm/min. However, this temperature is not high enough to enable inter-ply slip. As a consequence, fibrebuckling occurs at the inner bend section of the GF fabric/PEI laminates (fig. 4.27). Only at stamping temperatures of 265~ and above, which corresponds with a minimum stamping velocity of 300 mm/min, buckle-free vee-bend samples were produced.
4.3.5.3. Correlation between stamping velocity and stamping pressure 4.3.5.3.1. Influence of laminate stacking sequence Figure 4.28 shows the correlation between stamping velocity and stamping pressure in relation to the stacking sequence of CF/PP laminates. In this example, the switch-off pressure was set to 0.14 MPa. It is obvious that the resulting pressure increases with the stamping velocity. In addition, laminates with a higher number of 90 ~ layers lead to a reduced swing-over of the stamping pressure. This is caused by transverse flow in the 90 ~ layers in sample length direction [39]. The result is a remarkable reduction in the bend thickness (Ad/do) (fig. 4.29). For example, the thickness reduction at a stamping pressure of 2.5 MPa is 35% for [0~176 18% for [0~176176 but only 5% for a [0~ laminate. On the contrary, fibre transverse flow along the fibre direction does not occur in unidirectional laminates. Only a small amount of molten matrix is squeezed out in fibre direction. !
300 ~ I
~
~
t
s
i i
~
I /
I I
$ l:::
,--.,
0~
Stamping
velocity [ mm/min ]
A
206
0
600
.........
150
. . . . . . . . . . . . . . . . .
(D
"~ ~
100 50
i
~,
~--k'Ri
~
~:i
.... I
.................................................................................................................
0 0
20
40
60
80
1O0
Stamping time [ s ]
Fig. 4.26. Temperature profile of GF fabric/PEI laminate during stamp forming.
116
K. Friedrich et al.
Fig. 4.27. Fibre buckling at inner bend section of GF fabric/PEI laminate.
Fig. 4.28. Correlation between stamping velocity and stamping pressure in relation to laminate structure.
4.3.5.3.2. Influence o f fibre volume fraction The correlation of stamping velocity and pressure in unidirectional laminates as a function of fibre content and matrix material is shown in fig. 4.30. At the same switch-off pressure of 2.21MPa and stamping velocity of 300 mm/min, the resulting pressures are 4.5 MPa for CF/PP, 5.5 MPa for CF/PA12 and 6.5m MPa for C F / P E K laminates respectively. Due to the high fibre content in CF/PA12 and C F / P E E K laminates (60 vol. %), the rigidity of these two laminates is higher than that of the CF/PP laminates (only 20 vol. % CF) leading to higher pressure required for stamp forming process. The difference in
o f continuous f i b r e ~ t h e r m o p l a s t i c
Thermoforming
50
'
"
40 ._o r
30
-o r
I Z
1
aoo
|
_.,zl.....................................I
20
--
[]
10
t
~0f -
I '11
5o0
................................................. ~ ' ZX
[]
I*
400
..................................... 71 []
"0 oO
117
sheets
! Stamping velocity[ Laminate structure [ [mm/min] I 0]6 IEo,go,ol, lto,~O=ls " 100 .... E3
7-
-
t-
composite
I 01
o
I
zx
I
[]
9 I I
~
I
""
I
I
' .........
..Q c"
0 ore, 0
.................................................
i--,
............
"
-
"ID
rr
0
I
0
,
I
2
.
,
,
4
Stamping pressure [ MPa ]
i
6
,
8
Fig. 4.29. Thickness reduction of stamped bend side (stamping time: 10-15 s).
Fig. 4.30. Correlation between stamping velocity and stamping pressure in relation to matrix and fibre content.
stamping pressure between the CF/PA12 and CF/PEEK laminates can be explained by the different melting viscosities of the polymer matrix [34]. As already mentioned, the molten matrix can only migrate along the fibre direction during the forming of unidirectional laminates. This can lead to minor thickness reductions in the flat
l 18
K. Friedrich et al.
regions (fig. 4.31). At the same stamping pressure of 5 MPa, there is a reduction in leg thickness of 9% for CF/PP, 3% for CF/PA12 and 2% for CF/PEEK laminates. The sum of these results allows the conclusion that a greater reduction in thickness is linked to a higher matrix content and a lower viscosity of the molten polymer matrix. 4.3.5.3.3. Influence of laminate thickness Figure 4.32 shows the resulting stamping pressure as a function of GF fabric/PEI laminate thickness. The resulting
t Stamping velocity mm/min 200 PP CF2OO/o [] PAl2 .......
""
PAi2 PEEK
15
or) Or) t"
._o t,-
10
CF 40% CF60%
OF60% l ' J
[] []
f
9
300 6
400 9
500 I 9 I
~ *:
-X[]
~ I <> /
o
a
9
......
~ I" i & ! .Y'o ~ i i PA ~21'
,
f I
PA 12
". .O .. CO "rO
5
.,4
e.~
~-""el
_
~
K~..g~-t3"~l
to
,
o
-o
0
0
I 2
,
,
........
J
,
4 6 Stamping pressure [ MPa ]
i 8
Fig. 4.31. Influence of stamping pressure and stamping velocity on bend side thickness.
Fig. 4.32. Stamping pressure of GF/PEI laminate in relation to laminate thickness.
10
Thermoform&g of continuousfibre~thermoplastic composite sheets
119
stamping pressure decreases with increasing laminate thickness which can be explained as follows: (a) As the laminate thickness increases, the total number of plies that can slip over one another increases, too; however, increasing inter-ply slip reduces the stiffness of a laminate. (b) Thicker laminates have a greater thermal capacity than thinner ones. For this reason the stamping temperature of thicker laminates is higher than for thinner ones due to the slower cooling behaviour. Higher stamping temperatures also result in reduced stiffness of the laminate. Both factors can, in addition, reduce "swing-over" effects.
4.3.5.4. Effect of forming conditions on part geometry 4.3.5.4.1. Influence of stamping time on bend angle Additional to inter-ply slip between adjacent plies the fibres also have to bent in order to conform with the veeshape of the mould during forming. When re-heating a vee-bent part it tends to return to its original fiat state. This phenomenon is called memory or spring-back effect [29,40]. The magnitude of spring-back is mainly dependent on the stamping time (fig. 4.33). With a stamper radius of 2.5 mm and a stamping velocity of 400 mm/min, the following observations can be made for CF/PP laminates: 1. With increasing stamping time the discrepancy between mould angle (90 ~ and formed angle decreases. Here, a constant angle is achieved when the forming time exceeds 15 s, independent of the laminate's stacking sequence. 2. In a unidirectional laminate the spring-forward effect is not as strong as in laminates with 90 ~ layers. 3. In all parts, the formed angle is always smaller than the angle of the mould. 90
o
89
tl:l
o.
I
Laminate
I
[ 0 ] 6
structure '~
[0,90,0] s o I [ 0,902] s [] i ..............................................................................z~.................................................. ~ .....~..................................-.~--~................................... 2.5 mm
0 n CD t'-
Stamper radius
88
87
tH. ~
86
F0
,
0
, 10
i 20
, 30
stamping time [ s ] Fig. 4.33. Effect of stamping time on final angle of CF/PP laminate (stamping velocity: 400 mm/min;
stamping pressure: 3.26 MPa).
120
K. Friedrich et al.
In order to achieve a good conformity of the laminate's angle with the mould angle the fibres have to be arrested firmly in the matrix upon cooling. At short stamping times, with the matrix still being in its viscous state, elastic deformation of fibres cannot be prevented effectively resulting in a distorted cross-section of the vee-bent strips (fig. 4.34). This effect increased with decreasing forming times resulting in smaller effective bending angles of the parts. On the other hand, with increasing stamping time the cooling time of the stamped laminate is also extended, allowing the matrix to arrest the bent fibres resulting in a uniform angle. As mentioned earlier, 90 ~ layers in a laminate can lead to transverse flow of matrix and fibres. This effect can lead to an inhomogeneous distribution of 90 ~ layers in the fiat ends of the vee-bent parts, which is possibly the reason for not achieving a 90 ~ bend angle with these stacking sequences. Figure 4.35 illustrates the effect of stamping time and pressure on the final part angle of a [0~ laminate. For the various stamping pressures both bigger and more uniform angles were achieved with increasing stamping time. Uniform angles achieved with lower pressures are larger than that of higher stamping pressures. When stamping with a pressure of 3.26 MPa it takes about 15 s to form a uniform angle, whereas at a pressure of 5.53 MPa only 5 seconds are needed. Once a uniform angle is obtained the cross-sections of the strips do not exhibit any visible distortion as observed before (fig. 4.36). As mentioned in section 4.3.5.2, high stamping pressures lead to severe matrix flow between the fibre-rich layers in the bend resulting in excessive movement of the fibres near the bend region and consequently smaller part angles are obtained. The effect of the stamping time and mould geometry on the part angle formed at a pressure of 3.26 MPa and a velocity of 400 mm/min is illustrated in fig. 4.37. Again, the formed part angle increases with increasing stamping time reaching a constant value at stamping times in excess of 15 s. This result clearly depicts that the mould geometry, as used in this experiment, has no influence on the final angle of the veebent part. Similar dependencies of formed part angle on the stamping time were observed when forming GF/PP, CF/PA12 and C F / P E E K laminates.
.
.
.
.
d
Fig. 4.34. Schematic deformation of cross-section of bend side under short stamping time.
Thermoforming of continuous fibre/thermoplastic composite sheets
I
90
i
stamping velocity
9
El ll) o'J
89
stamping
1._.~
t,-
~
pressure
i
88
E2.
i
I
,!
i
[0]6
Laminate structure
121
400 mm/min 3.26 MPa
9
5.53 MPa
O
i t
i
"V"
t--
LL 87 t
I
86
....
0
I
10
Fig. 4.35. Final part angle of
[0]6
20
30
Stamping time [ s ]
CF/PP laminate in relation to stamping pressure and stamping time.
Pressure [Ml'a]
Press time
[s]
I
3.26
5.53
0.4
20.0
Fig. 4.36. Effect of stamping time on cross-section of bend side.
In contrast to the results obtained with unidirectional fibre reinforcements, the final part angle of GF fabric/PEI laminates as a function of the stamping time, with a stamping velocity of 700 mm/min, a pressure of 8.6 MPa and a stamper radius of 2.5 mm, is shown in fig. 4.38. Here, all angles are greater than the actual angle of the mould. Therefore, the following conclusions can be drawn: 1. The final angle obtained with fabric reinforcements is always greater than the actual angle of the mould. With increasing stamping times (more than 30 s) the resulting angles settle on a value close to 90 ~
122
K. Friedrich et al.
90
,
J
.,
Stamper radius [ mm]
9
2.5 5.0 10.0
89
Q
a
,..
88
0 r-! /k
! ~
. . . . . . . . . . . . . . . . . . . . . . . . .
T
~9
87
oEm
! 86
|
....
0
|
i
10
,,,
i
20
30
Stamping time [ s ] Fig. 4.37. Final part angle of
,~
98
[0]6
CF/PP laminate in relation to stamping time and stamper radius.
i
i
i
!
i
~TJ
a
96
i..~=
o) t-
! i i
....
i
!
I
94
i [.
i
[Warp,~ and [Weft]s
92 e.m
LL
9O 88
!..,. l i
10
"
.... - ! ,
,
i
.
2'-
[45~ ]s
20 Stamping time [ s ]
30
i
40
Fig. 4.38. Final part angle of GF fabric/PEI laminate in relation to stamping time (stamping velocity: 700 mm/min; stamping pressure: 8.6 MPa; stamper radius: 5.0 mm.
2. There is no differences observed between "weft" and "warp" stacked laminates under similar processing conditions. 3. The effect of stamping time on the formed angle decreases with increasing stamping radius. Looking at the structure of a woven fabric, the warp and weft yarns are interlaced tightly at their cross-over points; however, there is no physical bond between them. This interlocked structure does not allow transverse flow of warp or weft fibre
Thermoforming of continuousfibre~thermoplasticcompositesheets
123
bundles making it behave more like a sheet metal during forming. At very short stamping times the fabric reinforced laminates form greater angles but do not show a distortion of the cross-section of the bend legs. Due to the interlaced structure of a fabric the shear strength in warp and weft direction is low compared with the tensile and flexural strength in fibre direction. The shear strength is mainly resulting from the resistance to changes in the interlacing angle caused by friction and elastic restriction to the rotation of the interlacing angle between the warp and weft fibres [41]. In +45~ the fibres (warp and weft yarns) are orientated at an angle of 45 ~ to the stamper (fig. 4.39). The applied bending force not only leads to inter-ply shear between adjacent layers but also shear deformation between warp and weft and rotation of warp and weft in each individual layer. This way the spring-back of 45~ is hampered, making them less sensitive to stamping time and stamper radius than in laminates with "warp" and "weft" stacking sequence. In the stamp forming process described here, the deformed glass weave was kept in place through the change of phase of PEI matrix from molten and/or rubbery to glassy state. However, at very short stamping times (1-2 s), the temperature of the formed parts was still above the glass transition temperature of the PEI matrix during demoulding. Therefore, the matrix could not effectively prevent the tendency of the glass weave to spring back to its original fiat shape, leading to severe springback. On the contrary, at long stamping times (in excess of 30 s) the deformed glass weave was maintained by solidification of the polymer matrix under pressure. 4.3.5.4.2. Dependency of bending angle on other parameters Apart from the preheating temperature, the relationship between stamping velocity and pressure, the stamping time is another important forming parameter to be determined. Therefore, a series of stamp forming experiments employing different laminates' stacking sequences is described in the following paragraph. The angle measurement and optical examination of polished sections of the formed parts are utilised in order to assess the quality of the forming results.
Fig. 4.39. Deformationmechanismsof fabric-reinforcedlaminate.
124
K. Friedrich et al.
Figures 4.40 and 4.41 illustrate the effect of stamping velocity and pressure on the final part angle of stamp-formed CF/PP and G F / P P laminates at the example of three different laminate stacking sequences formed with a stamping time of 15-20 s. The optical inspection of a selection of parts shows that there are no voids to be observed in the bend region. However, none of the vee-bent parts measures an angle of exactly 90. On average, the reduction in angle is 2.0-4.0 ~ for CF/PP and 1.3-4.0 ~ for G F / P P laminates. In addition, for each laminate stacking sequence the angle reduction is also a function of stamping velocity and pressure, e.g. higher stamping velocities and pressures result in greater angle reductions. It has to be noted, that laminates with a higher number of 90 ~ plies exhibit more angle reduction and a bigger thickness reduction than unidirectional laminates. A microscopic inspection 90
89 a
9
o'J t--
Q.
stamping velocity Laminate str~cture [mm/min ] [ 0 ]61[ 0,90,0]s~[ 0.90: ]s 10o i / m 200 o 9 ................... .. 300 4, o [] 400 [] & " 500 o z~ ' ,, ~--..-~ -. ~-...........I ................
_ _ _
.....
_ _
88
87
t--
. ~
u_
86 0
2
4
6
8
Stamping pressure [ MPa ]
Fig. 4.40. Final part angle of CF/PP laminate in relation to stamping pressure and velocity. 90 a
L----.
' I I
I
89
. . . . . . . . . . . . . . . . . . . .
I i .......
l
0"} t.-
[0 6
. . . . . . . . . . . . . . . . .
[0,90,0] s
,--.=
Stamper radius[mm] h
I !
5-~
~
"
"
-i ,o0 j o . .
....
~
.... = l_1
-
88
[ 0,902]s ~ ~
c
"
[]
~
eA ~ ~ " " " ~ - . . ~ . L -
i
87
............................
U.
t .............................................
i
t
i
I
! 86
0
2
4
6
8
10
Stamping pressure [ MPa ]
Fig. 4.41. Final part angle of GF/PP laminate in relation to stamping pressure and velocity.
Thermoforming of continuousfibre~thermoplastic composite sheets
125
of some samples shows that, due to the transverse flow of fibre and matrix, the 90 ~ layers are not homogeneously distributed in the sample as in the flat laminate. The greater angle reduction in laminates with a high number of 90 ~ layers is believed to be associated with excessive transverse flow in these layers. The transverse flow mechanism in continuous-fibre-reinforced thermoplastics has been thoroughly studied by Barnes and Cogswell [39]. Additionally, it has been observed that the stamper radius has only little or negligible effect on the final part angle (fig. 4.41). The difference in angle between CF/PP and GF/PP laminate is thought to be associated with the properties of the different reinforcing fibres rather than the stamp radii. The effect of stamping velocity and pressure on the part angle of unidirectional laminates is summarised in fig. 4.42. Again, all angles are smaller than the actual angle of the mould (90~ The reduction of part angle increases with increasing stamping velocity and pressure for all materials. The angle reduction also increases with increasing matrix volume fraction. Applying the same stamping pressure, the matrix squeeze flow in CF/PP laminates (20 vol. %) is more extensive than in CF/ PAl2 (60 vol. %) and CF/PEEK (69 vol. %) laminates. Another reason for the differences in angles between CF/PA12 and CF/PEEK is thought to be associated with the different melting viscosities of the two polymers. Figure 4.43 illustrates the final part angle of GF fabric/PEI laminates as a function of stamper radius and laminate thickness. Here, the stamping pressure was set to 8.6 MPa with a velocity of 700 mm/min and a stamping time of 30--40 s. The laminates employed were either [warp]s or [weft]s. It is obvious that the formed part angle is not only dependent on the laminate thickness but also on the stamper radius; i.e. the spring-back effect decreases with increasing laminate thickness and stamper radius. The direct tool contact with the cold surface of the mould leads to a temperature gradient in the laminates consequently resulting in higher stamping temperatures in
9
e
stamping velocity PP PAl2 PAl2 PEEK mm/min CF 20% CF 40% CF 60% CF 60% 200 [] [] [] 9 300 o e 4, []
90 Dl::l:Zlg .....
a
....P A l 2 (
89
I
I
400
m
500
~
6
0
)
~
9
~
~-
isl
[]
<>
.........1.....................................................
" a A
9
I............................................. ,
r
"~ t~ 88 r-.
u_ 87
86 0
i
2
4 6 Stamping pressure [ MPa ]
I
8
]
10
Fig. 4.42. Final part angle of [0]s laminate in relation to stamping pressure and velocity.
126
K. Friedrich et al.
Fig. 4.43. Final part angle of GF fabric/PEI laminate in relation to stamper radius and laminate thickness (switch-off pressure: 2.08 MPa; stamping velocity: 700 mm/min). thicker laminates than in thinner ones. Keeping all stamping parameters constant, thicker laminates exhibit only little spring-back which explains the minor difference in mould to part angle. Another important factor influencing the spring-back is the local degree of deformation or the bend radius. When forming a large radius only little local deformation is needed to force the laminate into the cavity of the female mould meaning that only minor spring-back is observed. Figure 4.44 shows the polished cross-sections of G F fabric/PEI stamp formed samples with different stamper radii and laminate thicknesses.
Fig. 4.44. Section photomicrographs of bend samples made with different stamper radius (a) and laminate thickness (b).
Thermoforming of continuousfibre/thermoplastic composite sheets
127
4.3.5.4.3. Calculation of bending angle The results in section 4.3.5.4.2 showed that all the final part angles made from unidirectional laminates are smaller than the 90 ~ angle of the mould. This phenomenon is commonly called spring-forward effect [40] and is mainly the result of the anisotropy of thermal properties of composite materials. In particular, the difference between in-plane and out-of-plane thermal expansion coefficients is responsible for the discrepancy between the desired and actual shape of the stamped parts. Figure 4.45 shows two arc sections made from isotropic and anisotropic materials. Since the out-of-plane thermal expansion coefficient for an isotropic material is identical with the in-plane thermal expansion coefficient (Otr = d0), the thermal contraction of the arc section only results in minor
(~r
/
\\
/
// \\
//
// \ \ section / / \ \ \ \ angle / / / / \\ //
\ \
\ \
Xt
enclosed angle
(a)
a r = ~9
01 = 0 2
~r
/
/ /// / / / / / /
,
02 O1
(b)
a r > a 0 ,O1 >O2
Fig. 4.45. Thermally induced distortion in an arc section.
\
K. Friedrich et al.
128
changes of the arc's size. As a result, the section angle before and after thermal contraction remains constant (~1 = ~2) (fig. 4.45 (a)). In contrast, for anisotropic materials (in this case unidirectional fibre-reinforced composites) the out-of-plane thermal expansion coefficient is much higher than in in-plane direction (Otr>Oto). Therefore, during contraction of an anisotropic material the dimensions of the arc almost remain constant in one direction, whereas the other changes significantly. This results in a different arc size and hence a different configuration (fig. 4.45 b) which ultimately leads to the observed angle reduction. The thermal expansion coefficients of the unidirectional laminates employed for the experiments described here were determined by TMA. The results show that there is a remarkable difference between dr and c~0 (table 4.4). According to the mathematical studies by ONeill, the reduction in formed angle based on the anisotropy of the thermal properties can be calculated [42]. For simplicity, the angle section can be treated as being a sectional slice of a circular cylindrical tube. In this case it is then convenient to introduce polar co-ordinates (r, 0, z) as depicted in fig. 4.46. The following solutions can be then formulated:
(4.3.10)
u = u(r, 0), v = v(r, 0), w = w(r, O)
where u, v and w represent the r, 0 and z components of displacement in the circular section. The components of infinitesimal strain are then reduced to: Err
,u
~F ,
8zz = ~ Z '
,(,;)
EO0 - - - F
8r0---2
u-'l-
--~-~--~r--
(4.3.11)
F_.rz ~--- 80z = 0
TABLE 4.4 Thermal expansion coefficients of studied composite materials and estimated reduction in final part angle
Abbreviation
Vf (%)
CF/PP
GF/PP
Laminate structure
0/r (10-5K -1)
cto (10-6K -1)
AT (~
A ~ (degree)
20
[0]6 [0,90,0]s [0,902]s
17.9 20.0 20.6
2.6 4.8 7.3
135-140
2.1-2.2 2.3-2.5 2.4-2.6
33
[0]6 [0,90,0]s [0,902]s
14.2 14.0 14.5
12.5 7.2 9.8
135-140
1.5-1.7 1.6-1.7 1.6-1.7
14.0
-5.1
40 CF/PA12
[0]s 60
CF/PEEK
60
[01s
1.9-2.1 150-160
13